Phosphorized carbon nitride coated lithium manganese iron phosphate, preparation method thereof, positive electrode and battery

By phosphating carbon nitride coating lithium manganese iron phosphate, the Jahn-Teller effect of Mn3+ is suppressed, and the problems of conductivity and cycle life of lithium manganese iron phosphate materials in high-power applications are solved, achieving higher conductivity and cycle Performance improves the energy density and power density of the battery.

CN119008900APending Publication Date: 2024-11-22GEM CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411112427.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Lithium manganese iron phosphate material has reduced conductivity and poor cycle life in high-power applications, mainly due to the Jahn-Teller effect of Mn3+, causing Mn to precipitate, destroying the SEI film, and affecting the battery capacity and rate performance.

Method used

Carbon nitride phosphate (g-C3N4) is used to coat lithium manganese iron phosphate, and the P on the phosphate g-C3N4 structure is anchored with excessive metal elements in the lithium manganese iron phosphate phase, enhancing electron transport capability and inhibiting Mn Dissolution, improving conductivity and cycling properties.

Benefits of technology

The conductivity and cyclic properties of lithium manganese iron phosphate were significantly improved, with a discharge specific capacity of 0.1C reaching more than 146.4mAh/g, a discharge specific capacity of 1C reaching 133.7mAh/g, and a cyclic efficiency of 300 weeks under 1C conditions reached more than 99.2%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008900A_ABST
    Figure CN119008900A_ABST
Patent Text Reader

Abstract

The invention provides phosphatized carbon nitride coated lithium manganese iron phosphate and a preparation method thereof, a positive electrode and a battery. The phosphatized carbon nitride coated lithium manganese iron phosphate comprises lithium manganese iron phosphate core particles and a phosphatized carbon nitride material coating the outer sides of the lithium manganese iron phosphate core particles. The preparation method comprises the following steps: (1) mixing a lithium manganese iron phosphate raw material, a dispersing agent, an additive and a phosphatized carbon nitride material to obtain slurry; and (2) sequentially grinding, drying and sintering the slurry obtained in the step (1) to obtain the phosphatized carbon nitride coated lithium manganese iron phosphate. According to the invention, the electron transmission capability between the two can be obviously enhanced, the dissolution of Mn can be inhibited, and the conductivity and cycle performance of lithium manganese iron phosphate can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a carbon nitride phosphide coated lithium manganese iron phosphate and a preparation method thereof, a positive electrode and a battery. Background Art

[0002] As an upgraded product of lithium iron phosphate, lithium manganese iron phosphate contains manganese and iron in the material. This multi-element addition makes the battery design more flexible. The material shows some obvious advantages in energy density, low temperature performance, cost, etc. Lithium manganese iron phosphate has a higher dual-platform redox potential, and its energy density is 15% higher than that of lithium iron phosphate, which can meet the application requirements of high energy density and effectively alleviate the battery life anxiety. When it is paired with ternary materials, the capacity retention rate at -20°C can reach 70%. In addition, the relatively low cost also makes lithium manganese iron phosphate more attractive in low-cost applications.

[0003] However, lithium manganese iron phosphate also has some shortcomings. After the introduction of manganese, on the one hand, the conductivity of the material decreases, affecting the capacity and rate performance, and performing poorly in high-power applications; on the other hand, due to the Mn 3+ Due to the Jahn-Teller effect, Mn will precipitate and destroy the SEI film during the cycle, causing the battery capacity to decay and the cycle life to deteriorate. These shortcomings limit the large-scale application of lithium manganese iron phosphate in the market.

[0004] Although the existing carbon coating and nano-crystallization methods can improve the conductivity to a certain extent by shortening the diffusion path of electrons using small particle size, 3+ The degree of suppression of the Jahn-Teller effect is still low.

[0005] Therefore, it is urgent to develop new lithium manganese iron phosphate materials to inhibit Mn 3+ The Jahn-Teller effect. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a carbon nitride phosphide coated lithium manganese iron phosphate and a preparation method thereof, a positive electrode and a battery. By using g-C3N4 (carbon nitride phosphide) to coat the lithium manganese iron phosphate, the Mn 3+ The Jahn-Teller effect improves the conductivity and cycle performance of lithium manganese iron phosphate.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a carbon nitride phosphide coated lithium manganese iron phosphate, wherein the carbon nitride phosphide coated lithium manganese iron phosphate comprises a lithium manganese iron phosphate core particle and a carbon nitride phosphide material coated on the outside of the lithium manganese iron phosphate core particle.

[0009] The carbon nitride phosphide coated lithium manganese iron phosphate provided by the present invention is obtained by coating the carbon nitride phosphide material on the surface of the lithium manganese iron phosphate core particles, wherein g-C3N4 (carbon nitride) itself has high conductivity, and the P on the phosphide g-C3N4 structure can effectively anchor with the transition metal elements in the lithium manganese iron phosphate bulk phase, significantly enhancing the electron transmission capacity between the two and inhibiting Mn dissolution, thereby improving the conductivity and cycle performance of the lithium manganese iron phosphate.

[0010] Preferably, the carbon nitride phosphide material is a sheet-like material.

[0011] Preferably, the size of the phosphide carbon nitride material is 0.5-1 μm, for example, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm or 1 μm.

[0012] Preferably, P in the phosphide carbon nitride material is anchored to the transition metal in the lithium manganese iron phosphate core particles.

[0013] Preferably, the content of carbon phosphide nitride material in the carbon phosphide nitride coated lithium manganese iron phosphate is 0.4-1wt%, for example, it can be 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1wt%, etc.

[0014] Preferably, the particle size of the carbon nitride phosphide coated lithium manganese iron phosphate is 3 to 10 μm, for example, it can be 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or 10 μm, etc.

[0015] Preferably, the molar ratio of Mn:Fe in the carbon nitride phosphide coated lithium manganese iron phosphate is (1.5-3):1, for example, it can be 1.5:1, 1.7:1, 1.9:1, 2:1, 2.2:1, 2.4:1, 2.5:1, 2.7:1, 2.9:1 or 3:1, etc.

[0016] Preferably, the molar ratio of Li:(Mn+Fe) in the carbon nitride phosphide coated lithium manganese iron phosphate is (1-1.04):1, for example, it can be 1:1, 1.01:1, 1.02:1, 1.03:1 or 1.04:1.

[0017] In a second aspect, the present invention provides a method for preparing the carbon nitride phosphide coated lithium manganese iron phosphate according to the first aspect, the preparation method comprising the following steps:

[0018] (1) mixing raw materials of lithium iron manganese phosphate, a dispersant, an additive and a phosphating carbon nitride material to obtain a slurry;

[0019] (2) The slurry in step (1) is ground, dried and sintered in sequence to obtain the carbon nitride phosphide-coated lithium manganese iron phosphate.

[0020] The preparation method of the carbon nitride phosphide coated lithium manganese iron phosphate provided by the present invention is to add the carbon nitride phosphide material when mixing the raw materials of lithium manganese iron phosphate, which can be fully coated with the lithium manganese iron phosphate core particles; wherein the outer coating layer can improve the conductivity and electrochemical activity of the lithium manganese iron phosphate, thereby improving the performance of the electrode material, including higher discharge capacity and better cycle stability; further, the outer coated carbon nitride layer can provide an additional protective layer to prevent the lithium manganese iron phosphate from directly contacting the electrolyte, reducing the oxidation of the material and the corrosion of the electrolyte, thereby extending the service life of the electrode material. Moreover, carbon nitride, as a material with good conductivity, can effectively increase the diffusion rate of lithium ions in the electrode material. This helps to improve the reaction kinetics of the electrode material, reduce the resistance during the battery charge and discharge process, thereby improving the energy density and power density of the battery. Moreover, the P on the phosphated g-C3N4 structure can effectively anchor with the transition metal elements in the lithium manganese iron phosphate bulk phase, significantly enhancing the electron transmission capacity between the two and inhibiting the dissolution of Mn.

[0021] Compared with first preparing a lithium iron manganese phosphate precursor and then coating it, or first forming a lithium iron phosphate product and then coating it, the present invention needs to make full use of the interaction between the P on the g-C3N4 phosphide and the transition metal in the lithium iron manganese phosphate to inhibit the dissolution of Mn. Therefore, the method of adding g-C3N4 phosphide to the raw materials is adopted, so that the g-C3N4 phosphide material is not only coated on the outside of the crystalline lithium iron manganese phosphate, but the P therein also has a good anchoring effect with the internal transition metal elements.

[0022] Preferably, the preparation of the phosphated carbon nitride material comprises: mixing a carbon-nitrogen source and a first phosphorus source, and sequentially subjecting the mixture to calcination, particle refinement and ultrasound to obtain the phosphated carbon nitride material.

[0023] Preferably, the carbon-nitrogen source comprises urea and / or melamine.

[0024] The present invention further preferably uses urea and / or melamine as a carbon-nitrogen source, which can directly form C3N4 (carbon nitride), and then obtains a sheet-like phosphated carbon nitride material by ultrasonic stripping, which has better dispersion performance. The sheet-like phosphated carbon nitride material coated on the outside of lithium manganese iron phosphate can better improve the performance of the battery, and has broad application prospects.

[0025] Preferably, the first phosphorus source accounts for 0.05-10wt% of the total mass of the carbon-nitrogen source and the first phosphorus source, for example, it can be 0.05wt%, 1.16wt%, 2.27wt%, 3.37wt%, 4.48wt%, 5.58wt%, 6.69wt%, 7.79wt%, 8.9wt% or 10wt%, etc.

[0026] The present invention further preferably controls the content of the first phosphorus source within the above range, which can avoid the problem of insufficient connection strength between P and lithium manganese iron phosphate metal elements and poor ability to suppress the Jahn-Teller effect of the Mn element; at the same time, the amount of P anchored to the Mn metal of the lithium manganese iron phosphate body material is within a reasonable range, which will not affect the Li ion deintercalation process, and the final discharge specific capacity is high.

[0027] Preferably, the first phosphorus source comprises any one of diammonium phosphate, phosphoric acid or phosphorus pentoxide, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of diammonium phosphate and phosphoric acid, a combination of phosphorus pentoxide and phosphoric acid, and a combination of diammonium phosphate and phosphorus pentoxide.

[0028] Preferably, the calcination temperature is 450-600°C, for example, it may be 450°C, 467°C, 484°C, 500°C, 517°C, 534°C, 550°C, 567°C, 584°C or 600°C.

[0029] Preferably, the calcination time is 5 to 10 h, for example, 5 h, 5.6 h, 6.2 h, 6.7 h, 7.3 h, 7.8 h, 8.4 h, 8.9 h, 9.5 h or 10 h.

[0030] Preferably, the calcination is performed in an air atmosphere.

[0031] Preferably, the particle size of the particles after refinement is 50 to 100 nm, for example, it may be 50 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm or 100 nm.

[0032] Preferably, the power of the ultrasound is 100-600 W, for example, it can be 100 W, 105 W, 110 W, 200 W, 300 W, 400 W, 500 W or 600 W.

[0033] Preferably, the ultrasound time is 2 to 10 h, for example, 2 h, 2.9 h, 3.8 h, 4.7 h, 5.6 h, 6.5 h, 7.4 h, 8.3 h, 9.2 h or 10 h.

[0034] Preferably, the raw materials of the lithium manganese iron phosphate include a lithium source, an iron source, a manganese source and a second phosphorus source.

[0035] Preferably, the lithium source includes any one of lithium carbonate, lithium hydroxide, lithium nitrate, lithium chloride, lithium acetate or lithium dihydrogen phosphate, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of lithium carbonate and lithium hydroxide, a combination of lithium nitrate and lithium hydroxide, a combination of lithium carbonate and lithium nitrate, a combination of lithium chloride and lithium hydroxide, and a combination of lithium acetate and lithium dihydrogen phosphate.

[0036] Preferably, the iron source comprises any one of ferric phosphate, iron red, ferroferric oxide, ferric oxalate, ferric sulfate or ferric chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of ferric phosphate and iron red, a combination of ferric tetroxide and iron red, a combination of ferric phosphate and ferroferric oxide, a combination of ferric sulfate and iron red, and a combination of ferric phosphate and ferric chloride.

[0037] Preferably, the manganese source comprises any one of manganese dioxide, manganese pentoxide, trimanganese tetroxide, manganese carbonate, manganese oxalate or manganese hydrogen phosphate, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of manganese dioxide and manganese pentoxide, a combination of trimanganese tetroxide and manganese pentoxide, a combination of trimanganese tetroxide and manganese pentoxide, a combination of manganese hydrogen phosphate and trimanganese tetroxide, and a combination of manganese carbonate and manganese pentoxide.

[0038] Preferably, the second phosphorus source comprises any one of lithium dihydrogen phosphate, iron phosphate, phosphoric acid or ammonium dihydrogen phosphate, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of lithium dihydrogen phosphate and iron phosphate, a combination of phosphoric acid and iron phosphate, a combination of lithium dihydrogen phosphate and phosphoric acid, a combination of ammonium dihydrogen phosphate and iron phosphate, and a combination of lithium dihydrogen phosphate and ammonium dihydrogen phosphate.

[0039] Preferably, the raw material of lithium manganese iron phosphate also includes a carbon source.

[0040] Preferably, the carbon source accounts for 5-15% of the mass of the raw material of lithium manganese iron phosphate, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 8%, 9%, 9.5%, 10%, 11%, 12%, 13%, 14% or 15%, etc.

[0041] Preferably, the carbon source comprises any one of citric acid, glucose, starch or sucrose or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of citric acid and glucose, a combination of starch and glucose, a combination of citric acid and starch, a combination of sucrose and glucose, and a combination of citric acid and sucrose.

[0042] Preferably, the dispersant comprises any one of PEG, citric acid or oxalic acid or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of PEG and citric acid, a combination of oxalic acid and citric acid, and a combination of PEG and oxalic acid.

[0043] Preferably, the additive comprises any one of zirconium oxide, aluminum oxide, titanium oxide, magnesium oxide or niobium oxide, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of zirconium oxide and aluminum oxide, a combination of titanium oxide and aluminum oxide, a combination of zirconium oxide and titanium oxide, a combination of magnesium oxide and aluminum oxide, a combination of zirconium oxide and magnesium oxide, and a combination of niobium oxide and aluminum oxide.

[0044] Preferably, the mass ratio of the dispersant to the raw material of lithium iron manganese phosphate is 0.5-2%, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.5%, 1.8%, 1.9% or 2.0%, etc.

[0045] Preferably, the mass ratio of the additive to the raw material of lithium iron manganese phosphate is 0.2-1.2%, for example, it can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1% or 1.2%, etc.

[0046] Preferably, the mass ratio of the carbon nitride phosphide material to the raw material of lithium iron manganese phosphate is 0.8-2.5%, for example, it can be 0.8%, 0.9%, 1.0%, 1.2%, 1.3%, 1.4%, 1.5%, 1.8%, 2.0%, 2.2% or 2.5%, etc.

[0047] The present invention further preferably sets the mass ratio of the carbon nitride phosphide material to the raw material of lithium manganese iron phosphate within the above range, which can better balance the capacity of the bulk material and the effect of inhibiting the dissolution of the Mn element Jahn-Teller effect, and ultimately the overall electrochemical performance of the positive electrode material is better.

[0048] Preferably, the grinding rotation speed is 200-2000 rpm, for example, it can be 200 rpm, 400 rpm, 600 rpm, 800 rpm, 1000 rpm, 1200 rpm, 1400 rpm, 1600 rpm, 1800 rpm or 2000 rpm.

[0049] Preferably, the particle size after grinding is 200-400 nm, for example, it can be 200 nm, 220 nm, 250 nm, 280 nm, 300 nm, 310 nm, 320 nm, 350 nm, 380 nm or 400 nm.

[0050] Preferably, the grinding time is 3 to 10 h, for example, 3 h, 3.8 h, 4.6 h, 5.4 h, 6.2 h, 6.9 h, 7.7 h, 8.5 h, 9.3 h or 10 h.

[0051] Preferably, the drying in step (2) comprises spray drying.

[0052] Preferably, the sintering temperature is 650-800°C, for example, it may be 650°C, 667°C, 684°C, 700°C, 717°C, 734°C, 750°C, 767°C, 784°C or 800°C.

[0053] The present invention further preferably has a sintering temperature within the above range, which can better form a lithium iron manganese phosphate crystal phase with high crystallinity, while effectively ensuring the particle size range of the lithium iron manganese phosphate material.

[0054] Preferably, the sintering time is 8 to 15 hours, for example, it can be 8 hours, 8.8 hours, 9.6 hours, 10.4 hours, 11.2 hours, 11.9 hours, 12.7 hours, 13.5 hours, 14.3 hours or 15 hours.

[0055] Preferably, the sintering is performed under an inert atmosphere.

[0056] Preferably, the inert atmosphere comprises nitrogen and / or argon.

[0057] Preferably, the preparation method further comprises: the sintered sample is crushed, air flow crushed and iron removed in sequence to obtain the carbon nitride phosphide coated lithium manganese iron phosphate.

[0058] In a third aspect, the present invention provides a positive electrode, comprising the carbon nitride phosphide-coated lithium manganese iron phosphate as described in the first aspect.

[0059] The present invention has no special restrictions on other components and structures in the positive electrode. Any other components and structures that can be used in the positive electrode and are well known to those skilled in the art can be used, and can also be adjusted according to the actual process.

[0060] In a fourth aspect, the present invention provides a battery, comprising the positive electrode described in the third aspect.

[0061] The present invention has no special restrictions on other components and structures in the above-mentioned battery. Any other components and structures that can be used in batteries and are well known to those skilled in the art can be adopted, and can also be adjusted according to actual processes.

[0062] Compared with the prior art, the present invention has at least the following beneficial effects:

[0063] (1) The carbon nitride phosphide coated lithium manganese iron phosphate provided by the present invention is provided with a carbon nitride phosphide material on the surface of the lithium manganese iron phosphate core particles, wherein the P on the g-C3N4 phosphide structure can be effectively anchored with the transition metal elements in the lithium manganese iron phosphate bulk phase, significantly enhancing the electron transmission capacity between the two and inhibiting the dissolution of Mn, thereby improving the conductivity and cycle performance of the lithium manganese iron phosphate. Under preferred conditions, the 0.1C discharge specific capacity is above 146.4 mAh / g, the 1C discharge specific capacity reaches above 133.7 mAh / g, and the cycle efficiency of 300 cycles under 1C conditions reaches above 99.2%;

[0064] (2) The preparation method of carbon nitride phosphide coated lithium manganese iron phosphate provided by the present invention adds flaky phosphide g-C3N4 material to the raw material of lithium manganese iron phosphate. The phosphated C3N4 material, as an excellent electronic conductor, can be tightly and effectively coupled with the lithium manganese iron phosphate particles, thereby improving the electrical conductivity of the lithium manganese iron phosphate and inhibiting the dissolution of manganese, thereby promoting the improvement of its rate performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a SEM image of the flaky phosphated g-C3N4 material provided in Example 1 of the present invention.

[0066] Figure 2 This is a SEM image of carbon nitride phosphide coated lithium manganese iron phosphate provided in Example 1 of the present invention.

[0067] Figure 3 This is a graph showing the change in charge and discharge capacity after 300 cycles at 1C in Example 1 of the present invention. DETAILED DESCRIPTION

[0068] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0069] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0070] Example 1

[0071] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate, wherein the carbon nitride phosphide coated lithium manganese iron phosphate includes a lithium manganese iron phosphate core particle and a carbon nitride phosphide material coated on the outside of the lithium manganese iron phosphate core particle. P in the carbon nitride phosphide material is anchored to the transition metal in the lithium manganese iron phosphate core particle. The lithium manganese iron phosphate core particle is LiMn 0.7 Fe 0.3 PO4

[0072] The phosphated carbon nitride material is a flaky material, and the size D50 of the phosphated carbon nitride material is 100 nm; the content of the phosphated carbon nitride material in the phosphated carbon nitride coated lithium manganese iron phosphate is 0.4 wt%; and the particle size D50 of the phosphated carbon nitride coated lithium manganese iron phosphate is 6 μm.

[0073] This embodiment also provides a method for preparing the above-mentioned carbon nitride phosphide coated lithium manganese iron phosphate, the preparation method comprising the following steps:

[0074] (1) mixing a carbon-nitrogen source (melamine) and a first phosphorus source (specifically ammonium dihydrogen phosphate), wherein the first phosphorus source accounts for 5wt% of the total mass of the carbon-nitrogen source and the first phosphorus source, and sequentially calcining at 500°C for 8h, grinding to a particle size of 0.5 to 1 μm, and ultrasonicating in deionized water at 200W for 8h to obtain a phosphated carbon nitride material;

[0075] Mixing raw materials of lithium iron manganese phosphate (lithium carbonate, iron phosphate, manganese dioxide, lithium dihydrogen phosphate and glucose according to molecular formula), PEG, zirconium oxide and phosphide carbon nitride material to obtain slurry; wherein glucose accounts for 6% of the mass of the raw materials of lithium iron manganese phosphate; the mass ratio of PEG to the raw materials of lithium iron manganese phosphate is 1.5%; the mass ratio of zirconium oxide to the raw materials of lithium iron manganese phosphate is 0.4%; the mass ratio of phosphide carbon nitride material to the raw materials of lithium iron manganese phosphate is 0.8%;

[0076] (2) The slurry of step (1) is first ground at 500 rpm for 8 hours to a particle size of 200-400 nm, then spray-dried at 200° C., and sintered at 700° C. for 10 hours in an inert atmosphere (specifically, nitrogen atmosphere). The sintered sample is crushed, airflow-milled, and iron-removed in turn to obtain the carbon nitride phosphide-coated lithium manganese iron phosphate.

[0077] The phosphide carbon nitride material prepared in this embodiment 1 is as follows Figure 1 As shown, from Figure 1 It can be seen that the carbon nitride phosphide material is a flaky material and is evenly dispersed; the SEM image of the carbon nitride phosphide coated lithium manganese iron phosphate is as follows: Figure 2 As shown, from Figure 2 It can be seen that the carbon nitride phosphide coated lithium manganese iron phosphate obtained in the present invention has a uniform spherical structure.

[0078] Example 2

[0079] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate, wherein the carbon nitride phosphide coated lithium manganese iron phosphate includes a lithium manganese iron phosphate core particle and a carbon nitride phosphide material coated on the outside of the lithium manganese iron phosphate core particle. P in the carbon nitride phosphide material is anchored to the transition metal in the lithium manganese iron phosphate core particle. The lithium manganese iron phosphate core particle is LiMn 0.6 Fe 0.4 PO4

[0080] The phosphated carbon nitride material is a flaky material, and the size D50 of the phosphated carbon nitride material is 100 nm; the content of the phosphated carbon nitride material in the phosphated carbon nitride coated lithium manganese iron phosphate is 0.4 wt%; and the particle size D50 of the phosphated carbon nitride coated lithium manganese iron phosphate is 6 μm.

[0081] This embodiment also provides a method for preparing the above-mentioned carbon nitride phosphide coated lithium manganese iron phosphate, the preparation method comprising the following steps:

[0082] (1) mixing a carbon-nitrogen source (urea) and a first phosphorus source (specifically ammonium dihydrogen phosphate), wherein the first phosphorus source accounts for 10 wt% of the total mass of the carbon-nitrogen source and the first phosphorus source, and sequentially calcining at 450° C. for 10 h, grinding to a particle size of 0.5-1 μm, and ultrasonicating in deionized water at 200 W for 10 h to obtain a phosphated carbon nitride material;

[0083] Mixing raw materials of lithium iron manganese phosphate (lithium nitrate, ferroferric oxide, manganese tetraoxide, phosphoric acid and starch according to molecular formula), oxalic acid, titanium oxide and phosphide carbon nitride material to obtain slurry; wherein starch accounts for 6% of the mass of the raw materials of lithium iron manganese phosphate; the mass ratio of oxalic acid to the raw materials of lithium iron manganese phosphate is 1.5%; the mass ratio of titanium oxide to the raw materials of lithium iron manganese phosphate is 0.4%; the mass ratio of phosphide carbon nitride material to the raw materials of lithium iron manganese phosphate is 0.8%;

[0084] (2) The slurry of step (1) is first ground at 2000 rpm for 3 hours to a particle size of 200-400 nm, then spray-dried at 200° C., and sintered at 800° C. for 8 hours in an inert atmosphere (specifically, nitrogen). The sintered sample is crushed, airflow-milled, and iron-removed in turn to obtain the carbon nitride phosphide-coated lithium manganese iron phosphate.

[0085] Example 3

[0086] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate, wherein the carbon nitride phosphide coated lithium manganese iron phosphate includes a lithium manganese iron phosphate core particle and a carbon nitride phosphide material coated on the outside of the lithium manganese iron phosphate core particle. P in the carbon nitride phosphide material is anchored to the transition metal in the lithium manganese iron phosphate core particle. The lithium manganese iron phosphate core particle is LiMn 0.65 Fe 0.35 PO4

[0087] The phosphated carbon nitride material is a flaky material, and the size D50 of the phosphated carbon nitride material is 100 nm; the content of the phosphated carbon nitride material in the phosphated carbon nitride coated lithium manganese iron phosphate is 0.4 wt%; and the particle size D50 of the phosphated carbon nitride coated lithium manganese iron phosphate is 6 μm.

[0088] This embodiment also provides a method for preparing the above-mentioned carbon nitride phosphide coated lithium manganese iron phosphate, the preparation method comprising the following steps:

[0089] (1) mixing a carbon-containing nitrogen source (melamine) and a first phosphorus source (specifically ammonium dihydrogen phosphate), wherein the first phosphorus source accounts for 0.05wt% of the total mass of the carbon-containing nitrogen source and the first phosphorus source, and sequentially calcining at 600°C for 5h, grinding to a particle size of 0.5-1 μm, and ultrasonicating in deionized water at 200W for 2h to obtain a phosphated carbon nitride material;

[0090] Mixing raw materials of lithium iron manganese phosphate (lithium chloride, ferric sulfate, manganese carbonate, ammonium dihydrogen phosphate and sucrose according to molecular formula), citric acid, magnesium oxide and phosphide carbon nitride material to obtain slurry; wherein sucrose accounts for 6% of the mass of the raw materials of lithium iron manganese phosphate; the mass ratio of citric acid to the raw materials of lithium iron manganese phosphate is 1.5%; the mass ratio of magnesium oxide to the raw materials of lithium iron manganese phosphate is 0.4%; the mass ratio of phosphide carbon nitride material to the raw materials of lithium iron manganese phosphate is 0.8%;

[0091] (2) The slurry of step (1) is first ground at 200 rpm for 10 hours to a particle size of 200-400 nm, then spray-dried at 200° C., and sintered at 650° C. for 15 hours in an inert atmosphere (specifically, nitrogen). The sintered sample is crushed, airflow-milled, and iron-removed in turn to obtain the carbon nitride phosphide-coated lithium manganese iron phosphate.

[0092] Example 4

[0093] This embodiment provides a carbon nitride phosphide-coated lithium manganese iron phosphate, which is the same as Example 1 except that the first phosphorus source accounts for 15wt% of the total mass of the carbon-nitrogen source and the first phosphorus source, and will not be repeated here.

[0094] Example 5

[0095] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate, which is the same as Example 1 except that the first phosphorus source accounts for 0.01wt% of the total mass of the carbon-nitrogen source and the first phosphorus source, and will not be repeated here.

[0096] Example 6

[0097] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate. The carbon nitride phosphide coated lithium manganese iron phosphate is the same as that of Embodiment 1 except that ultrasound is not performed in step (1), and will not be described again.

[0098] Example 7

[0099] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate. The carbon nitride phosphide coated lithium manganese iron phosphate is the same as that of Embodiment 1 except that the mass ratio of the carbon nitride phosphide material to the raw material of the lithium manganese iron phosphate is 0.1%, and the rest is not repeated here.

[0100] Example 8

[0101] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate. The carbon nitride phosphide coated lithium manganese iron phosphate is the same as that of Embodiment 1 except that the mass ratio of the carbon nitride phosphide material to the raw material of the lithium manganese iron phosphate is 10%, and the details are not repeated here.

[0102] Example 9

[0103] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate. The carbon nitride phosphide coated lithium manganese iron phosphate is the same as that of Embodiment 1 except that it is sintered at 850° C. in step (2), and will not be described again.

[0104] Example 10

[0105] This embodiment provides a carbon nitride phosphide coated lithium manganese iron phosphate. Except for sintering at 600° C. in step (2), the carbon nitride phosphide coated lithium manganese iron phosphate is the same as that in embodiment 1, which will not be repeated here.

[0106] Comparative Example 1

[0107] This comparative example provides a carbon nitride-coated lithium manganese iron phosphate. The carbon nitride-coated lithium manganese iron phosphate is the same as Example 1 except that the first phosphorus source is not added in step (1), and the rest is not repeated here.

[0108] Comparative Example 2

[0109] This comparative example provides a lithium manganese iron phosphate, which is the same as Example 1 except that no phosphated carbon nitride is added and no phosphated carbon nitride is prepared in step (1), and the details are not repeated here.

[0110] Comparative Example 3

[0111] This comparative example provides a carbon phosphide nitride coated lithium manganese iron phosphate, which is the same as Example 1 except that carbon phosphide nitride is not added in step (1), but the spray-dried particles are mixed with carbon phosphide nitride after spray drying in step (2) and subsequently sintered. No further details are given here.

[0112] Comparative Example 4

[0113] This comparative example provides a fluorinated carbon nitride coated lithium manganese iron phosphate. The fluorinated carbon nitride coated lithium manganese iron phosphate is the same as Example 1 except that the first phosphorus source is not added in step (1) but is replaced by ammonium fluoride, and the rest is not repeated here.

[0114] The results of this test are all the results of the power-off test. The specific steps are as follows: weigh the positive electrode material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 and mix them in N-methylpyrrolidone (NMP); then, use a coater to apply the slurry on aluminum foil and dry it in a vacuum drying oven at 80°C for 8 hours. Finally, punch the aluminum foil into 1.13cm 2 The positive electrode sheet was obtained by forming a circular shape. The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and a porous polypropylene membrane (Celgard2400, USA) was used as a separator to separate the positive electrode and the counter electrode. The CR2032 button battery was assembled in an argon glove box. The cycle performance test was carried out at 2.5V-4.5V at a rate of 0.1C and 1C using a battery test system (Blue Electric CT2001A, Wuhan, China). The test results are shown in Table 1.

[0115] The battery assembled from the carbon nitride phosphide coated lithium manganese iron phosphate prepared in Example 1 has a 1C cycle performance as follows: Figure 3 As shown, from Figure 3 It can be seen that the positive electrode material obtained in Example 1 has excellent cycle performance, and the discharge specific capacity hardly decreases within 300 cycles.

[0116] The test results of the above embodiments and comparative examples are shown in Table 1.

[0117] Table 1

[0118]

[0119]

[0120] From Table 1, we can see the following points:

[0121] (1) It can be seen from Examples 1 to 3 that after the carbon nitride phosphide coated lithium manganese iron phosphate provided by the present invention forms a lithium ion battery, the 0.1C discharge specific capacity is above 146.4 mAh / g, the 1C discharge specific capacity reaches above 133.7 mAh / g, and the cycle efficiency of 300 weeks under 1C conditions reaches above 99.2%. The battery has excellent rate performance and cycle performance, and has broad application prospects.

[0122] (2) It can be seen from Example 1 and Examples 4 to 5 that the present invention controls the amount of the first phosphorus source added within a reasonable range, which can better improve the connection strength between P and lithium manganese iron phosphate metal elements and inhibit the Jahn-Teller effect of the Mn element, thereby improving the rate performance and cycle performance of the battery; at the same time, the amount of the first phosphorus source added is reasonably controlled to avoid excessive anchoring with the Mn metal of the lithium manganese iron phosphate main material, affecting the Li ion deintercalation process, and reducing the discharge specific capacity. Finally, the battery has a high discharge specific capacity and excellent battery performance;

[0123] (3) Combining Example 1 and Example 6, it can be seen that ultrasound is performed in step (1) of Example 1. After the positive electrode material of Example 1 is prepared into a lithium ion battery, the discharge specific capacity at 0.1C is 149.5 mAh / g; the discharge specific capacity at 1C is 139.2 mAh / g, and the cycle efficiency of 300 cycles under 1C is 99.2%. In Example 6, ultrasound is not performed, the size of the phosphated carbon nitride is larger, and the dispersibility is relatively low. The final discharge specific capacity at 0.1C is 137.6 mAh / g; the discharge specific capacity at 1C is 117.1 mAh / g, and the cycle efficiency of 300 cycles under 1C is 95.4%. This shows that the present invention can avoid agglomeration during the sintering process by preferably subjecting the phosphated carbon nitride to ultrasound treatment, thereby improving the discharge specific capacity and cycle efficiency of the lithium manganese iron phosphate material, and the electrochemical performance of the final material is better;

[0124] (4) It can be seen from Example 1 and Examples 7 to 8 that the mass ratio of the phosphide nitride carbon material to the raw material of lithium manganese iron phosphate in Example 1 is 0.8%, compared with 0.1% and 10% in Examples 7 to 8, respectively. After the positive electrode material in Example 1 is prepared into a lithium ion battery, the cycle efficiency of 300 weeks under 1C conditions is 99.2%; while the cycle efficiency of 300 weeks under 1C conditions in Examples 7 to 8 is 98.5% and 97%, respectively. This shows that the present invention can better inhibit the Jahn-Teller effect dissolution of the Mn element by adding a reasonable amount of phosphide nitride carbon material, and does not affect the capacity of the bulk material, thereby improving the comprehensive electrochemical performance;

[0125] (5) Combining Example 1 and Examples 9 to 10, it can be seen that the sintering temperature of step (2) in Example 1 is 700°C, compared with 850°C and 600°C in Examples 9 to 10, respectively. After the positive electrode material of Example 1 is prepared into a lithium ion battery, the discharge specific capacity at 0.1C is 149.5 mAh / g; the discharge specific capacity at 1C is 139.2 mAh / g, and the cycle efficiency of 300 cycles under 1C conditions is 99.2%; while the discharge specific capacity at 1C conditions in Example 9 is only 125.9 mA h / g, and the cycle efficiency of 300 weeks is only 92.5%. The discharge specific capacity at 1C under 1C in Example 10 is only 127.3 mAh / g, and the cycle efficiency of 300 weeks is only 95.8%. This shows that the present invention can better control the growth of lithium manganese iron phosphate particles containing phosphide carbon nitride by controlling the sintering temperature in step (2) within a reasonable range, avoid the increase of grain size and the lengthening of the lithium ion migration path, and at the same time ensure the crystallization performance of lithium iron phosphate, and finally improve the rate performance and cycle performance of the positive electrode material;

[0126] (6) It can be seen from Example 1 and Comparative Examples 1 to 4 that in Comparative Example 1, only carbon nitride is used for coating. Due to the lack of connection between P and the surface lattice of lithium manganese iron phosphate, the ability to suppress the Jahn-Teller effect of the Mn element becomes poor, and the 1C rate capacity and cycle performance of the material will decrease; in Comparative Example 2, no carbon nitride is added, and the final cycle efficiency of 300 cycles under 1C conditions is only 94.7%, and the cycle performance is significantly reduced; in Comparative Example 3, the phosphated carbon nitride and the precursor are directly mixed, and the contact between the phosphated carbon nitride and the precursor is poor, and the formed coating structure is poor, resulting in a decrease in the 1C discharge capacity of the material and a significant decrease in the cycle efficiency; in Comparative Example 4, fluorinated carbon nitride is used, which cannot achieve the effect of phosphating, and the final 1C discharge capacity of the material decreases to 123.2 mAh / g, and the cycle efficiency of 300 cycles is only 91.5%. This shows that the present invention can significantly improve the rate performance and cycle performance of the positive electrode material by coating lithium manganese iron phosphate with phosphated carbon nitride, and can also improve the discharge capacity.

[0127] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A carbon nitride phosphide coated lithium manganese iron phosphate, characterized in that: The carbon nitride phosphide coated lithium manganese iron phosphate comprises a lithium manganese iron phosphate core particle and a carbon nitride phosphide material coated on the outside of the lithium manganese iron phosphate core particle.

2. The carbon nitride phosphide coated lithium manganese iron phosphate according to claim 1, characterized in that: The phosphide carbon nitride material is a sheet material; Preferably, the size of the phosphide carbon nitride material is 0.5 to 1 μm; Preferably, the content of the carbon nitride phosphide material in the carbon nitride phosphide-coated lithium manganese iron phosphate is 0.4-1wt%; Preferably, the particle size of the carbon nitride phosphide coated lithium manganese iron phosphate is 3 to 10 μm; Preferably, the molar ratio of Mn:Fe in the carbon nitride phosphide coated lithium manganese iron phosphate is (1.5-3):1; Preferably, the molar ratio of Li:(Mn+Fe) in the carbon nitride phosphide coated lithium manganese iron phosphate is (1-1.04):

1.

3. A method for preparing carbon nitride phosphide coated lithium manganese iron phosphate according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) mixing raw materials of lithium iron manganese phosphate, a dispersant, an additive and a phosphating carbon nitride material to obtain a slurry; (2) The slurry in step (1) is ground, dried and sintered in sequence to obtain the carbon nitride phosphide-coated lithium manganese iron phosphate.

4. The preparation method according to claim 3, characterized in that: The preparation of the phosphated carbon nitride material comprises: mixing a carbon-nitrogen source and a first phosphorus source, and sequentially performing calcination, particle refinement and ultrasound to obtain the phosphated carbon nitride material; Preferably, the carbon-nitrogen source comprises urea and / or melamine; Preferably, the first phosphorus source accounts for 0.05-10 wt% of the total mass of the carbon-nitrogen source and the first phosphorus source; Preferably, the first phosphorus source includes any one of diammonium phosphate, phosphoric acid or phosphorus pentoxide, or a combination of at least two thereof.

5. The preparation method according to claim 4, characterized in that: The calcination temperature is 450-600°C; Preferably, the calcination time is 5 to 10 hours; Preferably, the calcination is carried out in an air atmosphere; Preferably, the particle size of the particles after refinement is 50 to 100 nm; Preferably, the power of the ultrasound is 100-600W; Preferably, the ultrasonication time is 2 to 10 hours.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The raw materials of the lithium manganese iron phosphate include a lithium source, an iron source, a manganese source and a second phosphorus source; Preferably, the raw material of lithium manganese iron phosphate also includes a carbon source; Preferably, the carbon source accounts for 5-15% of the raw material mass of lithium manganese iron phosphate; Preferably, the carbon source comprises any one of citric acid, glucose, starch or sucrose, or a combination of at least two thereof; Preferably, the mass ratio of the dispersant to the raw material of lithium manganese iron phosphate is 0.5-2%; Preferably, the mass ratio of the additive to the raw material of lithium manganese iron phosphate is 0.2-1.2%; Preferably, the mass ratio of the carbon nitride phosphide material to the raw material of lithium manganese iron phosphate is 0.8-2.5%.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The grinding speed is 200-2000 rpm; Preferably, the particle size after grinding is 200 to 400 nm; Preferably, the grinding time is 3 to 10 hours; Preferably, the drying in step (2) comprises spray drying; Preferably, the spray drying temperature is 180-240°C.

8. The preparation method according to any one of claims 3 to 7, characterized in that: The sintering temperature is 650-800°C; Preferably, the sintering time is 8 to 15 hours; Preferably, the sintering is carried out under an inert atmosphere; Preferably, the inert atmosphere comprises nitrogen and / or argon; Preferably, the preparation method further comprises: the sintered sample is sequentially crushed, air flow crushed and iron removed to obtain the carbon nitride phosphide coated lithium manganese iron phosphate.

9. A positive electrode, characterized in that: The positive electrode comprises the carbon nitride phosphide coated lithium manganese iron phosphate as claimed in claim 1 or 2.

10. A battery, characterized in that: The battery comprises the positive electrode according to claim 9.

Citation Information

Cited By

  • Preparation method of boronized carbon nitride composite lithium manganese iron phosphate positive electrode material

    CN120854528A

  • Positive electrode material and preparation method thereof, positive plate and secondary battery

    CN122051223A

  • Preparation method of phosphorus-doped graphite-phase carbon nitride coated manganese iron lithium phosphate

    CN122877730A