Sodium ferric phosphate pyrophosphate positive electrode material and preparation method thereof

By forming a carbon cladding layer on the surface of the positive electrode material of sodium ferric pyrophosphate, the mixture of organic and inorganic carbon sources is used to reduce the heterogeneous phases, the specific capacity and cycle stability of the sodium ferric pyrophosphate battery material are improved, and the existing technology is solved Performance problems caused by miscellaneous phase effects.

CN119008916AActive Publication Date: 2024-11-22HUNAN MEITE XINCAILIAO SCI & TECH CO LTD

Patent Information

Application Number
CN202411373963.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

The existing sodium ferric pyrophosphate battery materials have heterophasic phases due to process conditions, resulting in negative impacts on specific capacity and cycle stability.

Method used

A mixture of organic carbon source and inorganic carbon source is used as the carbon source to form a carbon cladding layer on the surface of the positive electrode material of sodium ferric pyrophosphate. A higher purified phase material is prepared by sintering, reducing the heterophasic content, improving specific capacity and cycling stability sex.

Benefits of technology

By controlling the types and proportions of carbon sources, a pure phase sodium ferrophosphate phosphate positive electrode material is achieved at a lower sintering temperature, which improves its specific capacity and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008916A_ABST
    Figure CN119008916A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a sodium ferric pyrophosphate positive electrode material. The chemical formula of the sodium ferric pyrophosphate positive electrode material is Na4Fe < 3 + x > (PO4) 2 (P2O7) (at) C, x is more than or equal to-0.3 and less than or equal to 0.3, C represents a carbon coating layer formed by the ferric sodium phosphate pyrophosphate positive electrode material, and in the preparation method, a source material carbon source of the carbon coating layer is a mixture of an organic carbon source and an inorganic carbon source. According to the preparation method of the sodium ferric phosphate pyrophosphate positive electrode material, the carbon source composed of the organic carbon source and the inorganic carbon source is sintered to form the carbon coating layer on the surface of the sodium ferric phosphate pyrophosphate positive electrode material, the types of the organic carbon source and the inorganic carbon source are selected, and the weight ratio of the organic carbon source to the inorganic carbon source is controlled; the high-purity-phase sodium ferric phosphate pyrophosphate positive electrode material is prepared, the content of impure phases is reduced, the specific capacity and the first effect of the sodium ferric phosphate pyrophosphate positive electrode material are improved, and the positive electrode material has favorable influence on cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of battery positive electrode materials, and in particular to a sodium iron phosphate pyrophosphate positive electrode material and a preparation method thereof. Background Art

[0002] In sodium ion battery materials, in order to allow sodium ions to obtain a larger diffusion channel in the crystal, stabilize the crystal structure, and improve the electrochemical performance of the electrode material, PO4 3- , P2O7 4- Etc. are introduced into the electrode material system, and this type of material is collectively called polyanions.

[0003] Pyrophosphate has the advantages of high energy density and high power density. Compared with sulfate and phosphate, it has higher thermal stability and relatively easy preparation process, making it the polyanion material with the performance closest to practical application. At present, sodium iron pyrophosphate phosphate products on the market are affected by process conditions and basically have a small amount of impurities such as sodium iron phosphate and sodium iron pyrophosphate, which leads to serious negative impact on the specific capacity and cycle stability of sodium iron pyrophosphate battery materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a sodium iron phosphate pyrophosphate positive electrode material and a preparation method thereof.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a sodium iron phosphate pyrophosphate positive electrode material, wherein the chemical formula of the sodium iron phosphate pyrophosphate positive electrode material is Na4Fe 3+x (PO4)2(P2O7)@C; -0.3≤x≤0.3, C represents the carbon coating layer formed by the sodium iron phosphate pyrophosphate positive electrode material;

[0006] In the preparation method, the carbon source of the source material of the carbon coating layer is a mixture of an organic carbon source and an inorganic carbon source, the organic carbon source is at least one of lauric acid, sodium laurate, and maltodextrin, and the inorganic carbon source is at least one of graphite emulsion and Ketjen black; the weight ratio of the organic carbon source to the inorganic carbon source is 1: (0.3~3).

[0007] The above-mentioned method for preparing sodium iron phosphate pyrophosphate positive electrode material forms a carbon coating layer on the surface of the sodium iron phosphate pyrophosphate positive electrode material by sintering using a carbon source composed of an organic carbon source and an inorganic carbon source, and selects the types of the organic carbon source and the inorganic carbon source and controls the weight ratio of the organic carbon source and the inorganic carbon source to prepare a relatively pure sodium iron phosphate pyrophosphate positive electrode material, reduces the content of the impurity phase, improves the specific capacity and the first effect of the sodium iron phosphate pyrophosphate positive electrode material, and has a favorable effect on the cycle stability. And the pure sodium iron phosphate pyrophosphate positive electrode material can be obtained at a lower sintering temperature.

[0008] Preferably, the sodium iron phosphate pyrophosphate positive electrode material is prepared from an iron source, a sodium source, a phosphorus source and a carbon source.

[0009] Preferably, the weight content of the carbon coating layer in the sodium iron pyrophosphate positive electrode material is 0.5% to 3%.

[0010] Preferably, the organic carbon source in the carbon source is maltodextrin and the inorganic carbon source is Ketjen black.

[0011] In the above-mentioned method for preparing the sodium iron phosphate pyrophosphate positive electrode material, when the organic carbon source in the carbon source is maltodextrin and the inorganic carbon source is Ketjen black, the specific capacity and cycle stability of the sodium iron phosphate pyrophosphate positive electrode material are better.

[0012] Preferably, the preparation method comprises the following steps:

[0013] (1) mixing an iron source, a dispersant, a sodium source, a phosphorus source and a carbon source in deionized water and grinding the mixture in a sand mill;

[0014] (2) spray drying the liquid after sand milling in step (1) to obtain a precursor mixed powder;

[0015] (3) ball milling the precursor mixed powder of step (2);

[0016] (4) sintering the precursor mixed powder of step (3) at 500-550° C. for 8-15 h in an inert gas atmosphere to obtain a sodium iron pyrophosphate positive electrode material;

[0017] (5) Grinding the sodium iron phosphate pyrophosphate positive electrode material in step (4) by air flow.

[0018] The method for preparing the sodium iron phosphate pyrophosphate positive electrode material adopts wet mixing followed by spray drying, and the carbon source is mixed together in the wet mixing step, and ball milling is performed after spray drying, so that the sodium iron phosphate pyrophosphate positive electrode material prepared after sintering is purer.

[0019] Preferably, in step (1), the dispersant accounts for 0.5wt% to 10wt% of the total weight of the iron source, dispersant, sodium source, phosphorus source and carbon source, and the dispersant is at least one of PVA, PEG, PVB and CMC.

[0020] Preferably, in step (1), the average particle size of the particles after sand grinding is controlled to be 0.5 to 2 μm.

[0021] Preferably, in step (1), the sand mill speed for sand grinding is 1000-1400 rpm, and the sand grinding time is 3-6 hours.

[0022] Preferably, in step (2), the inlet air temperature of the spray drying is 220-260° C., the outlet air temperature is 110-140° C., the atomization pressure is 0.3-0.5 MPa, and the feed speed is 20 rpm-40 rpm.

[0023] Preferably, in step (3), the ball-to-material ratio of ball milling is (6-25):1.

[0024] Preferably, the sodium source is at least one of sodium carbonate, sodium bicarbonate, sodium acetate, sodium citrate, disodium hydrogen phosphate, disodium hydrogen citrate, and sodium hydroxide.

[0025] Preferably, the phosphorus source is at least one of phosphoric acid, sodium dihydrogen phosphate, trisodium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, and monosodium trihydrogen pyrophosphate.

[0026] Preferably, the iron source is ferric phosphate, ferrous oxalate dihydrate or ferric oxide.

[0027] Preferably, in the carbon source, the ratio of the organic carbon source to the inorganic carbon source is 1:(0.6-2).

[0028] The present invention also provides a sodium iron phosphate pyrophosphate positive electrode material prepared by any of the above-mentioned sodium iron phosphate pyrophosphate positive electrode material preparation methods.

[0029] The beneficial effects of the present invention are as follows: the present invention provides a sodium iron phosphate pyrophosphate positive electrode material and a preparation method thereof. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention forms a carbon coating layer on the surface of the sodium iron phosphate pyrophosphate positive electrode material by sintering using a carbon source composed of an organic carbon source and an inorganic carbon source, and selects the types of the organic carbon source and the inorganic carbon source and controls the weight ratio of the organic carbon source and the inorganic carbon source, thereby preparing a sodium iron phosphate pyrophosphate positive electrode material with a relatively high purity phase, reducing the content of the impurity phase, improving the specific capacity and the first efficiency of the sodium iron phosphate pyrophosphate positive electrode material, and having a favorable effect on the cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the XRD diagram of the sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention.

[0031] Figure 2 This is the XRD diagram of the sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention.

[0032] Figure 3 This is the XRD diagram of the sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention.

[0033] Figure 4This is the XRD diagram of the sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material in the comparative example of the present invention.

[0034] Figure 5 This is the XRD diagram of the sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material in the comparative example of the present invention. DETAILED DESCRIPTION

[0035] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0036] Example 1

[0037] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the chemical formula of the sodium iron phosphate pyrophosphate positive electrode material is Na4Fe 3+x (PO4)2(P2O7)@C; x = -0.15, C represents the carbon coating layer formed by the sodium iron pyrophosphate positive electrode material;

[0038] The preparation method comprises the following steps:

[0039] (1) After the iron source, dispersant, sodium source, phosphorus source and carbon source are uniformly mixed in deionized water, the solid-liquid ratio of the solid-liquid material is 18g solid phase material to 92mL water; sand milling is performed; the carbon source accounts for 3wt% of the weight of all source materials of the iron source, sodium source, phosphorus source and carbon source; the carbon source is a mixture of an organic carbon source and an inorganic carbon source, and the ratio of the organic carbon source to the inorganic carbon source is 1:1; the dispersant accounts for 0.5wt% of the total weight of the iron source, dispersant, sodium source, phosphorus source and carbon source, and the dispersant is polyvinyl alcohol (PVA); the sand mill speed of the sand mill is 1200rpm, the sand milling time is 4h, and the average particle size of the particles after sand milling is controlled to be 0.5-2μm; the sodium source is sodium carbonate, the phosphorus source is sodium dihydrogen phosphate, and the iron source is ferrous oxalate dihydrate; the organic carbon source in the carbon source is maltodextrin, and the inorganic carbon source is graphite emulsion;

[0040] (2) spray drying the liquid after sand milling in step (1) to obtain a precursor mixed powder; the spray drying has an inlet air temperature of 240° C., an outlet air temperature of 120° C., an atomization pressure of 0.4 MPa, and a feed speed of 30 rpm;

[0041] (3) ball milling the precursor mixed powder of step (2); the ball-to-material ratio of ball milling = (6-25):1;

[0042] (4) heating the precursor mixed powder of step (3) to 520° C. in an inert gas atmosphere and sintering for 10 h to obtain a sodium iron phosphate pyrophosphate positive electrode material;

[0043] (5) Grinding the sodium iron phosphate pyrophosphate positive electrode material in step (4) by air flow.

[0044] Example 2

[0045] As a method for preparing sodium iron phosphate pyrophosphate positive electrode material according to an embodiment of the present invention, the only difference between this embodiment and embodiment 1 is that the organic carbon source in the carbon source is lauric acid, and the inorganic carbon source is Ketjen black.

[0046] Example 3

[0047] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material according to an embodiment of the present invention, the only difference between this embodiment and embodiment 1 is that the organic carbon source in the carbon source is maltodextrin, and the inorganic carbon source is Ketjen black.

[0048] Example 4

[0049] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the only difference between this embodiment and Example 3 is that the organic carbon source in the carbon source is maltodextrin, the inorganic carbon source is Ketjen black, and the weight ratio of maltodextrin to Ketjen black is 1.5:1.

[0050] Example 5

[0051] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the only difference between this embodiment and Example 3 is that the organic carbon source in the carbon source is maltodextrin, the inorganic carbon source is Ketjen black, and the weight ratio of maltodextrin to Ketjen black is 2:1.

[0052] Example 6

[0053] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the only difference between this embodiment and Example 3 is that the organic carbon source in the carbon source is maltodextrin, the inorganic carbon source is Ketjen black, and the weight ratio of maltodextrin to Ketjen black is 2.5:1.

[0054] Example 7

[0055] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the only difference between this embodiment and Example 3 is that the organic carbon source in the carbon source is maltodextrin, the inorganic carbon source is Ketjen black, and the weight ratio of maltodextrin to Ketjen black is 1:1.5.

[0056] Example 8

[0057] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material in an embodiment of the present invention, the only difference between this embodiment and Example 3 is that the organic carbon source in the carbon source is maltodextrin, the inorganic carbon source is Ketjen black, and the weight ratio of maltodextrin to Ketjen black is 1:2.

[0058] Comparative Example 1

[0059] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material as a comparative example of the present invention, the only difference between this comparative example and Example 3 is that the carbon source is an organic carbon source, and the organic carbon source is maltodextrin.

[0060] Comparative Example 2

[0061] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material as a comparative example of the present invention, the only difference between this comparative example and Example 3 is that the carbon source is an inorganic carbon source, and the inorganic carbon source is Ketjen black.

[0062] Comparative Example 3

[0063] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material as a comparative example of the present invention, the only difference between this comparative example and Example 3 is that the organic carbon source in the carbon source is glucose, and the inorganic carbon source is Ketjen black.

[0064] Comparative Example 4

[0065] As a method for preparing a sodium iron phosphate pyrophosphate positive electrode material as a comparative example of the present invention, the only difference between this comparative example and Example 3 is that the organic carbon source in the carbon source is maltodextrin, and the inorganic carbon source is conductive carbon black.

[0066] Experimental methods

[0067] 1. Samples to be tested

[0068] The polyvinyl alcohol used in the experiment is polyvinyl alcohol 17-88 type, with a molecular weight of 10000-50000. The remaining materials are all chemical materials of analytical grade or higher. According to the methods of Examples 1-8 and Comparative Examples 1-4, the sodium iron pyrophosphate positive electrode material is prepared, and the total amount of raw materials of the iron source, dispersant, sodium source, phosphorus source and carbon source is prepared after mixing according to 5g. As the sample to be tested.

[0069] 2. Phase purity detection

[0070] Test method: Perform XRD test on the prepared samples, and fit the test data using Fullprof software to obtain the content of different phases.

[0071] XRD test was performed on the sodium iron phosphate pyrophosphate positive electrode materials of Examples 1 to 3 and Comparative Examples 1 to 2. The experimental results are as follows: Figure 1 to Figure 5 As shown, Figure 1 This is a result diagram of the sodium iron phosphate pyrophosphate positive electrode material of Example 1, wherein Figure 2 This is a result diagram of the sodium iron phosphate pyrophosphate positive electrode material of Example 2, wherein Figure 3 This is a result diagram of the sodium iron phosphate pyrophosphate positive electrode material of Example 3, wherein Figure 4 This is the result diagram of the sodium iron phosphate pyrophosphate positive electrode material of Comparative Example 1, wherein Figure 5 This is the result diagram of the sodium iron pyrophosphate positive electrode material of Comparative Example 2.

[0072] It can be seen that the method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention can prepare a sodium iron phosphate pyrophosphate positive electrode material with a relatively high phase purity. As shown in Table 1, it is the test result of the purity of the sodium iron phosphate pyrophosphate positive electrode material of the present invention.

[0073] Table 1 Test results of purity of sodium iron pyrophosphate positive electrode material

[0074]

[0075] 3. Specific capacity and cycle stability test

[0076] Test method: The positive electrode sheet made of the obtained positive electrode composite material (85wt%), Super P conductive carbon black (5wt%), and polyvinylidene fluoride (10wt%) is used as the positive electrode of the sodium ion battery, and the metal sodium sheet is used as the counter electrode. 5vol.% of fluoroethylene carbonate is added to the NaClO4 / propylene carbonate solution with a concentration of 1mol / L as the electrolyte, and glass fiber is used as a diaphragm. It is assembled into a button battery in a high-purity argon atmosphere glove box. Using the constant current charge and discharge mode, the charge and discharge test is carried out at a current density of 0.1C for 5 weeks, and then changed to a high rate of 1C to characterize its rate performance and cycle performance. The test conditions are: the discharge cut-off voltage is 2.0V, and the charge cut-off voltage is 4.0V

[0077] The experimental results are shown in Table 2.

[0078] Table 2 Specific capacity and cycle stability of sodium iron pyrophosphate positive electrode materials

[0079]

[0080]

[0081] As can be seen from Table 2, the method for preparing the sodium iron phosphate pyrophosphate positive electrode material of the present invention forms a carbon coating layer on the surface of the sodium iron phosphate pyrophosphate positive electrode material by sintering using a carbon source composed of an organic carbon source and an inorganic carbon source, and selects the types of the organic carbon source and the inorganic carbon source and controls the weight ratio of the organic carbon source and the inorganic carbon source. The prepared sodium iron phosphate pyrophosphate positive electrode material with a higher pure phase reduces the content of the impurity phase and improves the specific capacity and cycle stability of the sodium iron phosphate pyrophosphate positive electrode material. In particular, when the organic carbon source in the carbon source is maltodextrin and the inorganic carbon source is Ketjen black, the phase of the prepared sodium iron phosphate pyrophosphate positive electrode material is purer, which improves the specific capacity and cycle stability of the sodium iron phosphate pyrophosphate positive electrode material.

[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a sodium iron pyrophosphate positive electrode material, It is characterized in that The chemical formula of the sodium iron phosphate pyrophosphate positive electrode material is Na 4 Fe 3 +x(PO 4 ) 2 (P 2 O 7 )@C; -0.3≤x≤0.3, C represents the carbon coating layer formed by the sodium iron pyrophosphate positive electrode material; In the preparation method, the carbon source of the source material of the carbon coating layer is a mixture of an organic carbon source and an inorganic carbon source, the organic carbon source is at least one of lauric acid, sodium laurate, and maltodextrin, and the inorganic carbon source is at least one of graphite emulsion and Ketjen black; the weight ratio of the organic carbon source to the inorganic carbon source is 1: (0.3~3).

2. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 1, It is characterized in that The weight content of the carbon coating layer in the sodium iron phosphate pyrophosphate positive electrode material is 0.5% to 3%.

3. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 1, It is characterized in that The organic carbon source in the carbon source is maltodextrin and the inorganic carbon source is Ketjen black.

4. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 1, It is characterized in that The preparation method comprises the following steps: (1) mixing an iron source, a dispersant, a sodium source, a phosphorus source and a carbon source in deionized water and grinding the mixture in a sand mill; (2) spray drying the liquid after sand milling in step (1) to obtain a precursor mixed powder; (3) ball milling the precursor mixed powder of step (2); (4) sintering the precursor mixed powder of step (3) at 500-550° C. for 8-15 h in an inert gas atmosphere to obtain a sodium iron pyrophosphate positive electrode material; (5) Grinding the sodium iron phosphate pyrophosphate positive electrode material in step (4) by air flow.

5. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 4, It is characterized in that In step (1), the dispersant accounts for 0.5wt% to 10wt% of the total weight of the iron source, dispersant, sodium source, phosphorus source and carbon source, and the dispersant is at least one of PVA, PEG, PVB and CMC.

6. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 4, It is characterized in that In step (1), the average particle size of the particles after sand grinding is controlled to be 0.5 to 2 μm.

7. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 4, It is characterized in that In step (2), the inlet air temperature of the spray drying is 220-260° C., the outlet air temperature is 110-140° C., the atomization pressure is 0.3-0.5 MPa, and the feed speed is 20 rpm-40 rpm; in step (3), the ball-to-material ratio of the ball mill is (6-25):

1.

8. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 4, It is characterized in that The sodium source is at least one of sodium carbonate, sodium bicarbonate, sodium acetate, sodium citrate, disodium hydrogen phosphate, disodium hydrogen citrate, and sodium hydroxide; the phosphorus source is at least one of phosphoric acid, sodium dihydrogen phosphate, trisodium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium pyrophosphate, trisodium monohydrogen pyrophosphate, disodium dihydrogen pyrophosphate, and monosodium trihydrogen pyrophosphate; the iron source is ferric phosphate, ferrous oxalate dihydrate, or ferric oxide.

9. The method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to claim 4, It is characterized in that In the carbon source, the ratio of the organic carbon source to the inorganic carbon source is 1:(0.6-2).

10. The sodium iron phosphate pyrophosphate positive electrode material prepared by the method for preparing the sodium iron phosphate pyrophosphate positive electrode material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Double-coated lithium iron phosphate cathode material and preparation method thereof

    CN109888281A

  • Positive electrode material for sodium-ion battery and preparation method of positive electrode material

    CN112447947A

  • Preparation method of lithium iron phosphate positive electrode material with long cycle life

    CN115566160A

  • Preparation method of phosphate-based polyanionic compound and application of phosphate-based polyanionic compound in sodium-ion battery

    CN116344752A

  • Modified high-nickel ternary positive electrode material, preparation method thereof and lithium ion battery

    CN116995215A

Cited By

  • Pyrophosphate ferric sodium phosphate as well as preparation method and application thereof

    CN120039844A

  • Modified ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN120964755A

  • Polyanion composite positive electrode material and preparation method thereof

    CN120978049A

  • Sodium ferric phosphate pyrophosphate positive electrode material, preparation method thereof and sodium ion battery

    CN121565860A

  • A sodium iron pyrophosphate cathode material and its preparation method, and its application in sodium-ion batteries.

    CN121565860B