High-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode catalyst and preparation method thereof
By preparing RuO2/Co3O4/NiO porous nanosheet composite materials, the kinetics and stability issues of cathode catalysts in lithium-oxygen batteries were solved, achieving efficient oxygen reduction and oxygen evolution catalysis, improving the specific capacity and cycle life of the battery, simplifying the preparation process, reducing costs, and making it suitable for large-scale applications.
Patent Information
- Application Number
- CN202411093708.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing lithium-oxygen battery cathode catalysts suffer from problems such as slow oxygen reduction and oxygen evolution reaction kinetics, numerous side reactions, limited cycle life, low actual energy density, and high charge-discharge overpotential. Furthermore, current preparation methods are lengthy and costly, making commercial application difficult.
A RuO2/Co3O4/NiO porous nanosheet composite material was prepared using a glucose template method. By utilizing the spontaneous electron transfer and strong coupling effect at the heterogeneous interface of the three-phase composite material, the formation pathway of discharge products was regulated. Combined with the nanoporous structure, the transport of electrolyte and gas was accelerated, thereby improving catalytic activity and stability.
It achieves efficient dual-function catalysis for oxygen reduction and oxygen evolution, significantly improving the specific capacity and cycle life of lithium-oxygen batteries, simplifying the preparation process, reducing costs, and making it suitable for large-scale applications.
Smart Images

Figure CN119008978A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemistry and new energy technology, and specifically relates to a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode catalyst and a preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Since the Industrial Revolution, the large-scale use of fossil energy has promoted the process of global industrialization and also brought about environmental pollution. Therefore, the application of green, low-carbon, safe and efficient energy systems has become a research hotspot. At present, among the various energy storage and conversion devices, lithium-ion batteries are the most widely used secondary battery systems, but they are limited by their low theoretical energy density and are difficult to meet the future society's demand for large-scale smart grids. Lithium-oxygen batteries can directly use oxygen that is easily available in the environment as an electrode active substance and have an extremely high theoretical energy density (~3500Wh kg -1 ), low material cost and environmental friendliness and has attracted widespread attention from all over the world.
[0004] However, lithium-oxygen batteries are still in the early stages of development, and some technical problems still need to be overcome to achieve commercial application. Among them, the slow kinetics of oxygen reduction and oxygen evolution reactions on the cathode side of lithium-oxygen batteries and the accompanying side reactions are the main factors leading to the low rate performance, limited cycle life, small actual energy density and high charge / discharge overpotential of lithium-oxygen batteries. Therefore, designing and developing efficient bifunctional cathode catalysts with reasonable structures is an effective way to solve the above problems.
[0005] At present, the research on efficient cathode catalyst materials has accumulated for decades. Precious metal-based catalysts are widely used in the field of electrocatalysis due to their excellent catalytic activity. Among them, the precious metal oxide RuO2 exhibits excellent oxygen evolution catalytic activity and good conductivity, which can significantly accelerate the reaction kinetics and improve the reaction activity. Li et al. only used porous RuO2 hollow spheres as the cathode catalyst of lithium-oxygen batteries (FJLi, DMTang, T.Zhang, KMLiao, P.He, D.Golberg, A.Yamada, HSZhou, Superior Performance of a Li-O2 Battery with Metallic RuO2 Hollow Spheres as the Carbon-Free Cathode, Advanced Energy Materials 2015, 5, 1500294). In the limited voltage window of 2.30-4.00V and the current density of 100mA g -1 Under the test conditions, the reversible charge / discharge specific capacity obtained is about 1400 mAh g -1 , the charge / discharge overpotential is as low as 0.54 / 0.13V respectively, at 500mAg -1 Zhang et al. designed hydrangea-like RuO2 mesoporous materials as positive electrode catalysts for lithium-oxygen batteries (CF Zhang, DMTang, XK Hu, XZ Liu, T. Zhang, H. S Zhou, Scalable Synthesis and Excellent Catalytic Effect of Hydrangea-like RuO2 Mesoporous Materials for Lithium-O2 Batteries, Energy Storage Materials 2016, 2, 8). -1 Under the test conditions, it can achieve about 1000mAh g -1The reversible charge / discharge specific capacity is only 3.36 / 2.78V. After 100 cycles of full charge / discharge, the charge overpotential only increases by 0.23V, and the discharge overpotential remains at 0.18V. Guo et al. encapsulated RuO2 nanoparticles in nanoporous nitrogen-doped graphene as a positive electrode catalyst for lithium-oxygen batteries (XW Guo, P. Liu, JH Han, Y. Ito, A. Hirata, T. Fujita, MW Chen, 3D Nanoporous Nitrogen-Doped Graphene with Encapsulated RuO2 Nanoparticles for Li-O2 Batteries, Advanced Materials 2015, 27, 6137). In the limited voltage window of 2.20-4.25V and the current density of 200mAg -1 Under the test conditions, it can achieve about 8700mAh g -1 The reversible charge / discharge capacity at a current density of 400 mAg -1 , cut-off specific capacity is 2000mAh g -1 Under the condition of , a cycle life of more than 100 times can be achieved. However, the abundance of precious metals in the earth's crust is low and their prices are high, which seriously restricts their large-scale application. Transition metal oxides have become the most promising substitutes for precious metal catalysts due to their excellent electrochemical activity, abundant resource reserves, low prices and simple preparation process.
[0006] Among many transition metal oxides, spinel Co3O4 is not only easy to synthesize and has controllable structure and morphology, but also exhibits outstanding oxygen reduction catalytic activity and stability. Cui et al. deposited Co3O4 on nickel foam as a positive electrode catalyst for lithium-oxygen batteries (YM Cui, ZY Wen, Y. Liu, A Free-Standing-Type Design for Cathodes of Rechargeable Li-O2 Batteries, Energy & Environmental Science 2011, 4, 4727). -2 Under the same conditions, the discharge voltage is kept above 2.91V and the discharge capacity exceeds 4000mAh g -1, while the charging voltage can be maintained between 3.40-3.50 V. Zhang et al. designed hierarchical porous Co3O4 nanoboxes as cathode catalysts for lithium-oxygen batteries (J. Zhang, Z. Y. Lyu, F. Zhang, L. J. Wang, P. Xiao, K. D. Yuan, M. Lai, W. Chen, Facile Synthesis of Hierarchical Porous Co3O4 Nanoboxes as Efficient Cathode Catalysts for Li-O2 Batteries, Journal of Materials Chemistry A 2016, 4, 6350), with a limited voltage window of 2.00-4.50 V and a current density of 0.08 mA cm -2 Under the condition of -1 The reversible charge / discharge specific capacity at a current density of 0.16 mA cm -2 、Cut-off specific capacity 1000mAhg -1 Jiang et al. used Co3O4 nanoflower materials as lithium oxygen battery catalysts (ZL Jiang, GL Xu, Z. Yu, TH Zhou, WK Shi, CSLuo, HJ Zhou, LB Chem, WJS Heng, MX Zhou, L. Cheng, RS Assary, SG Sun, K. Amine, H. Sun, High Rate and Long Cycle Life in Li-O2 Batteries with Highly Efficient Catalytic Cathode Configured with Co3O4 Nanoflower, Nano Energy 2019, 64, 103896). In the limited voltage window of 2.00-4.30 V and the current density of 100 mA g -1 Under the condition of , the charge / discharge specific capacity can reach 13430 / 15702mAh g -1 , the coulombic efficiency can reach 87% at a current density of 1000mA g -1 , cut-off specific capacity is 1000mAh g -1Under the conditions of , an ultra-long cycle life of more than 248 times can be achieved. It is worth noting that NiO, as a p-type semiconductor, not only has the characteristics of a wide band gap, diverse structural morphology, good thermal stability and safety, but has also been proven to be able to efficiently decompose by-products during the charge and discharge cycle of lithium-oxygen batteries to avoid the accumulation of passivation layers. Misun et al. loaded hexagonal nanoporous NiO on carbon nanotubes as a positive electrode catalyst for lithium-oxygen batteries to improve the oxidation efficiency of by-products such as lithium carbonate and lithium carboxylate (M. Hong, HC Choi, HRByon, Nanoporous NiO Plates with A Unique Role for Promoted Oxidation of Carbonate and Carboxylate Species in the Li-O2 Battery, Chemistry of Materials 2015, 27, 2234). At a current density of 250 mA g -1 、Cut-off specific capacity 1000mAh g -1 Under the test conditions, a cycle life of more than 70 times was achieved. Mu et al. used rapid laser scanning technology to prepare dense nano-villous NiO containing oxygen vacancies on nickel foam and used it as a positive electrode catalyst for lithium-oxygen batteries (XWMu, QHWen, G.Ou, YMDu, P.He, MLZhong, H.Zhu, H.Wu, SXYang, YJLiu, BJLi, XPZhang, HSZhou, A Current Collector Covering Nanostructured Villous Oxygen-Deficient NiO Fabricated by RapidLaser-Scan for Li-O2 Batteries, Nano Energy 2018, 51, 83). In the limited voltage window of 2.00-4.30V and the current density of 100mAg -1 Under the test conditions, about 500mAh g was obtained at a lower charging potential (3.84V). -1The reversible charge / discharge specific capacity is 73.5% of the initial specific capacity after 100 cycles of full charge and discharge. Long et al. synthesized P-doped nanoflower-shaped NiO by hydrothermal method and subsequent annealing method and used it as a positive electrode catalyst for lithium-oxygen batteries (YXLong, ZD Zhang, LL Zhao, QX Zeng, Q.Li, J.Wang, DY Li, Q.Xia, Y.Liu, X.Han, ZR Zhou, YB Li, YM Zhang, SL Chou, Bucket Effect on High-Performance Li-O2Batteries Based on P-doped 3D NiO Microspheres with Conformal Growth ofDischarge Products, Journal of Materials Chemistry A2022, 10, 24538). The specific capacity of NiO nanoflower-shaped ... -1 Under the test conditions, the charge / discharge specific capacity can reach 16490 / 16628mAh g -1 The charge / discharge overpotential is 1.05 / 0.29V at a current density of 500mA g -1 , cut-off specific capacity is 600mAh g -1 Under the test conditions, an ultra-long cycle life of more than 300 times can be achieved. However, both Co3O4 and NiO have the disadvantages of low electrical conductivity and limited oxygen evolution catalytic activity, which need to be improved by combining with other catalysts with good conductivity.
[0007] In addition, although the current research on multiphase metal oxide lithium oxygen battery positive electrode catalysts has made certain progress, the related preparation methods currently reported have lengthy processes, high economic costs, and do not show catalytic effects that meet current expectations, and cannot be widely used in actual production. Summary of the invention
[0008] In order to solve the above problems, the present invention provides a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode catalyst and a preparation method thereof. The obtained RuO2 / Co3O4 / NiO porous nanosheet is a three-phase composite material formed by RuO2, Co3O4, and NiO. Due to the difference between the Fermi levels of the three, the electrons at the heterogeneous interface spontaneously transfer across the interface, thereby adjusting the electronic structure of the composite material and enhancing its conductivity. In addition, the strong coupling between the multiphases changes the adsorption capacity of the composite material for the reaction intermediates, effectively regulating the formation path of the discharge product lithium peroxide, thereby improving the specific capacity and cycle life of the lithium oxygen battery. Secondly, the constructed heterogeneous structure can trigger a slight lattice distortion through the Jahn-Teller effect, forming a disordered atomic arrangement to provide additional electrochemical reaction active sites, thereby improving the catalytic performance of the material. In addition, the interconnected nanoporous structure has abundant pores and a large three-dimensional space, which can effectively accelerate the transmission of gas and electrolyte during the charge / discharge process, is conducive to the storage of discharge products, and realizes the improvement of cycle performance and rate performance.
[0009] In order to achieve the above object, the present invention adopts the following technical solution:
[0010] The first aspect of the present invention provides a method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst, comprising:
[0011] Preparing a mixed solution of ruthenium salt, cobalt salt and nickel salt, wherein the molar ratio of ruthenium salt, cobalt salt and nickel salt is 10-30:40-80:10-50;
[0012] RuO2 / Co3O4 / NiO porous nanosheets were prepared using a mixed solution of ruthenium salt, cobalt salt and nickel salt as raw materials and a glucose template method.
[0013] The present invention combines RuO2, Co3O4 and NiO to effectively enhance the oxygen evolution ability, conductivity and stability of the catalyst, develops a high-efficiency bifunctional catalyst with both oxygen reduction and oxygen evolution, and achieves a dual consideration of low economic cost and high catalytic activity research and development of the catalyst.
[0014] In some embodiments, the specific steps of the glucose template method include:
[0015] Glucose and urea are added to a mixed solution of ruthenium salt, cobalt salt and nickel salt, mixed evenly, and calcined to obtain the product.
[0016] The purpose of using the glucose template method in the present invention is to utilize the gas released by the decomposition of urea in high-temperature molten glucose syrup to promote the uniform loading of metal salts on the glucose porous template, and finally form porous nano-sheet oxides with uniform distribution of metal elements under high-temperature calcination.
[0017] In order to avoid the deposition of impurity atoms affecting product quality. Therefore, in some embodiments, the ruthenium salt is ruthenium trichloride hydrate;
[0018] In some embodiments, the cobalt salt is cobalt chloride hexahydrate;
[0019] In some embodiments, the nickel salt is nickel chloride hexahydrate.
[0020] In some embodiments, the glucose is anhydrous glucose, and the solvent is deionized water.
[0021] In some embodiments, the molar ratio of urea to glucose is 3-5:5-7.
[0022] In some embodiments, the concentration of the ruthenium source in the mixed solution is 10-30 mmol L -1 The concentration of cobalt source is 40-80mmol L -1 The concentration of nickel source is 10-50mmol L -1 , the concentration of urea is 3-5 mol L -1 , the concentration of glucose is 5-7 mol L -1 ;
[0023] Preferably, in the mixed solution, the concentration of urea is 3.33 mmol L -1 , the concentration of glucose is 5.55mmolL -1 ;
[0024] In some embodiments, the calcining is performed under an air atmosphere.
[0025] In some embodiments, the calcination is divided into two times.
[0026] In some embodiments, the first calcination temperature is 120-160° C. and the calcination time is 6-10 h, so that the urea in the molten glucose syrup can be fully decomposed, which is conducive to the subsequent formation of a porous nanosheet-shaped final product;
[0027] In some embodiments, the second calcination temperature is 400-600° C., and the calcination time is 10-14 h.
[0028] Preferably, the heating rate of the calcination is 3-5°C min -1 .
[0029] More specifically, they include:
[0030] adding glucose and urea to a mixed solution of ruthenium salt, cobalt salt and nickel salt to obtain a uniform mixed solution;
[0031] The mixed solution is transferred into a crucible and placed in a muffle furnace, and calcined twice in an air atmosphere to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0032] The second aspect of the present invention provides a RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode catalyst prepared by the above method.
[0033] In some embodiments, the RuO2 / Co3O4 / NiO porous nanosheets present a three-dimensional sheet structure in which nanoparticles are uniformly interconnected. The particle size of the nanoparticles is 10-30 nm, and the width of the three-dimensional nanosheets is 1-5 μm. The specific surface area of the RuO2 / Co3O4 / NiO porous nanosheet positive electrode catalyst material is 8-26.1585 m 2 g -1 ;
[0034] The third aspect of the present invention provides the use of the above-mentioned RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode catalyst in the preparation of a positive electrode of a lithium oxygen battery or a lithium oxygen battery.
[0035] In some embodiments, the positive electrode of a lithium oxygen battery is prepared using the above-mentioned RuO2 / Co3O4 / NiO porous nanosheet, including a positive electrode catalyst material, a conductive agent, a binder and a current collector, and the positive electrode catalyst material is the above-mentioned high-performance RuO2 / Co3O4 / NiO porous nanosheet.
[0036] In some embodiments, the preparation method is to add the positive electrode catalyst material, the conductive agent, and the binder into an organic solvent and mix them evenly to obtain an electrode slurry, apply the electrode slurry on the surface of the current collector, and dry it;
[0037] Preferably, the mass ratio of the positive electrode catalyst material, the conductive agent, and the binder is 3.5-4.5:3.5-4.5:1.5-2.5.
[0038] In some embodiments, the lithium oxygen battery is prepared using the above-mentioned lithium oxygen battery positive electrode, wherein the lithium oxygen battery includes a positive electrode, a negative electrode, a separator and an electrolyte, and the positive electrode catalytic material in the positive electrode is the above-mentioned high-performance RuO2 / Co3O4 / NiO porous nanosheet.
[0039] Beneficial effects of the present invention
[0040] (1) The present invention adopts a simple glucose template method to prepare a RuO2 / Co3O4 / NiO heterostructure composite material with porous nanosheets. The preparation process is simple, green and pollution-free, with high yield and large-scale application. It can provide effective impetus for the industrial production and large-scale application of lithium-oxygen batteries.
[0041] (2) The added glucose provides a template for the uniform distribution of metal salts. The amount of urea added affects the structure of the glucose template and the growth morphology of the material. Changing the amount of ruthenium salt, cobalt salt and nickel salt added can affect the ratio of RuO2, Co3O4 and NiO in the material, thereby affecting the catalytic performance of the material in lithium-oxygen batteries. The temperature and time of the first calcination will affect the decomposition rate of urea and thus affect the porous structure of the glucose template. The particle size of RuO2 / Co3O4 / NiO nanoparticles and the size and crystallinity of the porous nanosheets formed by the interconnection are all related to the temperature and time of the second calcination.
[0042] (3) The three-dimensional sheet structure prepared by the present invention is nanoscale and has abundant three-dimensional pores, which can significantly promote the transmission of electrolyte and gas, provide space for storing discharge products, and reduce volume expansion during the charge / discharge process, thereby ensuring the integrity of the electrode structure during the cycle.
[0043] (4) The composite material with rich heterogeneous interfaces constructed by the present invention has a large number of additional active sites and built-in electric fields. The electronic structure at the specific heterogeneous interface can effectively promote the transmission of electrons and strengthen the coupling and synergistic effect between the various parts, which can effectively regulate the generation path of discharge products and improve the specific capacity and cycle stability of the material.
[0044] (5) The RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery positive electrode prepared by the present invention exhibits high cycle stability and specific capacity. In a specific embodiment, the catalyst is -1 Under the current density and 2.35-4.35 V voltage window conditions, it shows lower charging and higher discharging platforms (3.65 and 2.74 V), as well as lower charge / discharge overpotentials (0.69 / 0.22 V), and the first charge / discharge specific capacity can reach 16632.0 / 16634.5 mAh g -1 , Coulomb efficiency exceeds 99%; the charge / discharge terminal voltage changes little with the increase of current density, and has good rate performance; at a current density of 500mA g -1 , fixed specific capacity 600mAh g -1 Under the test conditions, more than 180 cycles can be achieved at a current density of 200 mAg -1 , fixed specific capacity 600mAh g -1 Under the test conditions, it can stably cycle more than 110 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute improper limitations on the present invention.
[0046] Figure 1 is the XRD pattern of the RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1;
[0047] Figure 2 This is the FESEM image of the RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1;
[0048] Figure 3 The EDS-Mapping spectrum of the RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1, wherein (a) is the corresponding FESEM image of RuO2 / Co3O4 / NiO, (b) is the EDS-Mapping element summary image of RuO2 / Co3O4 / NiO, (c) is the mapping image of the O element, (d) is the mapping image of the Ru element, (e) is the mapping image of the Co element, and (f) is the mapping image of the Ni element;
[0049] Figure 4 TEM image of RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1;
[0050] Figure 5 HRTEM images of the RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1, wherein (a) is a HRTEM image, and (b), (c), and (d) are enlarged images of the area shown in (a);
[0051] Figure 6 This is a BET specific surface area test diagram of the RuO2 / Co3O4 / NiO porous nanosheets prepared in Example 1;
[0052] Figure 7 This is a performance diagram of the first cycle of charge / discharge test of the RuO2 / Co3O4 / NiO porous nanosheet prepared in Example 1 for lithium oxygen battery testing;
[0053] Figure 8 The RuO2 / Co3O4 / NiO porous nanosheet prepared in Example 1 is used in the rate test performance of lithium oxygen battery, with current density of 200, 300, 400, 500, 600, 200 mA g -1 ;
[0054] Fig. 9The RuO2 / Co3O4 / NiO porous nanosheet prepared in Example 1 is used in the cycle performance test of lithium oxygen battery. The test conditions are: current density 500mA g -1 、Cut-off specific capacity 600mAh g -1 ;
[0055] Fig.10 The RuO2 / Co3O4 / NiO porous nanosheet prepared in Example 1 is used in the cycle performance test of lithium oxygen battery. The test conditions are: current density 200mA g -1 、Cut-off specific capacity 600mAh g -1 . DETAILED DESCRIPTION
[0056] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0057] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0058] Example 1
[0059] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0060] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0061] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0062] Figure 1XRD test results of RuO2 / Co3O4 / NiO porous nanosheets synthesized in this embodiment. The diffraction data are consistent with RuO2 (JCPDS No.40-1290), Co3O4 (JCPDS No.43-1003) and NiO (JCPDS No.78-0643), and no impurity phase appears, indicating that the product is a high-purity RuO2 / Co3O4 / NiO material; Figure 2 This is a FESEM image of the RuO2 / Co3O4 / NiO porous nanosheet synthesized in this example. The material as a whole presents a porous sheet structure, and the surface presents protruding nanoparticles; Figure 3 This is the EDS-Mapping spectrum of the RuO2 / Co3O4 / NiO porous nanosheet synthesized in this example. It can be seen that ruthenium, cobalt, nickel and oxygen elements are evenly distributed on the surface of the material; Figure 4 The TEM image of the RuO2 / Co3O4 / NiO porous nanosheet synthesized in this embodiment shows that the RuO2 / Co3O4 / NiO composite material synthesized in this invention presents a three-dimensional sheet structure of interconnected nanoparticles as a whole, and the size of the nanoparticles is about 15nm; Figure 5 They are HRTEM images of the RuO2 / Co3O4 / NiO porous nanosheets synthesized in this embodiment, respectively. It can be concluded that the RuO2 / Co3O4 / NiO porous nanosheets synthesized in this invention are heterogeneous structural composite materials in which RuO2, Co3O4 and NiO coexist in three phases; Figure 6 The BET specific surface area test diagrams of RuO2 / Co3O4 / NiO nanoporous nanosheets synthesized in this embodiment are respectively shown. The specific surface area of the sample is measured to be 26.1585 m 2 g -1 .
[0063] The RuO2 / Co3O4 / NiO porous nanosheets obtained in Example 1 were used to prepare electrodes in the following manner:
[0064] RuO2 / Co3O4 / NiO porous nanosheets, carbon black and PTFE were weighed in a mass ratio of 4:4:2, and an appropriate amount of isopropanol solution was added. The suspension was ultrasonically dispersed to obtain an electrode material slurry, which was then evenly coated on a circular carbon paper with a diameter of 19 mm to form an electrode, and then dried in a vacuum drying oven at 120°C for 12 h. A 2032-type button cell with holes was used for the electrochemical test of lithium-oxygen batteries. A metal lithium sheet was used as the negative electrode, and 1 mol L -1 LiNO3 / DMSO solution, Whatman GF / D glass fiber was used as the separator. The battery assembly was carried out in a glove box filled with argon atmosphere, and the electrochemical test was carried out using LAND CT2001A multi-channel battery tester in a pure oxygen environment at room temperature.
[0065] Figure 7 The material obtained in this example is used as a positive electrode catalyst for lithium oxygen batteries at 200mA g -1 The battery performance under the test conditions of current density and cutoff voltage of 2.35-4.35V showed that the battery exhibited lower charging and higher discharging platforms (3.65 and 2.74V), as well as lower charge / discharge overpotentials (0.69 / 0.22V). The specific capacity of the first charge / discharge could reach 16632.0 / 16634.5mAh g -1 , Coulombic efficiency exceeds 99%; Figure 8 The material obtained in this example is used as a rate performance test diagram of a positive electrode catalyst for a lithium-oxygen battery. The results show that the charge / discharge terminal voltage changes little with the increase of current density, and has good rate performance; Fig. 9 The cycle performance diagram of the material obtained in this example as a positive electrode catalyst for a lithium oxygen battery is shown in Figure 2. -1 、Current density 600mAg -1 Under the condition of , the charge / discharge test can obtain more than 180 times of excellent cycle performance; Fig.10 The material obtained in this example is used as a lithium oxygen battery positive electrode catalyst cycle performance diagram, at a current density of 200mAg -1 , fixed specific capacity 600mAh g -1 Under the test conditions, the charge / discharge test can obtain an excellent cycle performance of more than 110 times.
[0066] Example 2
[0067] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0068] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0069] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 120℃ and kept at this temperature for 8h, and then continued to rise at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0070] Example 3
[0071] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0072] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0073] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 160°C at a rate of 1.5°C / min and kept at that temperature for 8 h. -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0074] Example 4
[0075] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0076] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0077] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature is raised to 400°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0078] Example 5
[0079] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0080] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0081] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature is raised to 600 °C at a rate of 100 °C and kept at this temperature for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0082] Example 6
[0083] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0084] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0085] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 6h, and then continued at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0086] Example 7
[0087] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0088] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0089] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 10h, and then continued to rise at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0090] Example 8
[0091] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0092] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0093] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 10 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0094] Example 9
[0095] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0096] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.3mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0097] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature was raised to 500 °C at a rate of 100 °C and kept at this temperature for 14 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0098] Example 10
[0099] The preparation method of RuO2 / Co3O4 / NiO porous nanosheets comprises the following steps:
[0100] S1. Prepare the reaction solution: add 0.1mmol of ruthenium trichloride hydrate, 0.1mmol of cobalt chloride hexahydrate and 0.1mmol of nickel chloride hexahydrate into 5mL of deionized water, and stir magnetically for 10min to obtain a uniform mixed solution. Then, add 1g of urea and 5g of anhydrous glucose into the above solution in sequence, and stir magnetically for 30min to obtain a uniform and transparent mixed solution;
[0101] S2. Preparation of RuO2 / Co3O4 / NiO porous nanosheets: The uniform transparent mixed solution obtained in step S1. was transferred into a crucible and placed in a muffle furnace in an air atmosphere at 3°C min -1 The temperature was raised to 140℃ and kept at this temperature for 8h, and then continued at 3℃min -1 The temperature is raised to 500°C at a heating rate and kept for 12 h, and then naturally cooled to room temperature to obtain RuO2 / Co3O4 / NiO porous nanosheets.
[0102] Comparative Example 1
[0103] The difference from Example 1 is that no ruthenium trichloride hydrate was added.
[0104] The material obtained in this comparative example is used as a positive electrode catalyst for lithium oxygen batteries at 200mA g -1 Under the test conditions of current density and cutoff voltage of 2.35-4.35V, the specific capacity of the battery for the first charge / discharge is 5965.4 / 7229.0mAh g -1, the coulombic efficiency is 82.5%; at a fixed specific capacity of 500mAh g -1 、Current density 600mAg -1 The charge / discharge test was carried out under the condition of 47 cycles; at the current density of 200mA g -1 , fixed specific capacity 600mAh g -1 The charge / discharge test was carried out under the test conditions and only 16 cycle performances were obtained.
[0105] Comparative Example 2
[0106] The difference from Example 1 is that cobalt chloride hexahydrate is not added.
[0107] The material obtained in this comparative example is used as a positive electrode catalyst for lithium oxygen batteries at 200mA g -1 Under the test conditions of current density and cutoff voltage of 2.35-4.35V, the specific capacity of the battery for the first charge / discharge is 11155.1 / 12703.9mAh g -1 , the coulombic efficiency is 87.8%; at a fixed specific capacity of 500mAh g -1 、Current density 600mA g -1 The charge / discharge test was carried out under the condition of 109 cycles; at the current density of 200mA g -1 , fixed specific capacity 600mAh g -1 The charge / discharge test was carried out under the test conditions and 61 cycle performances were obtained.
[0108] Comparative Example 3
[0109] The difference from Example 1 is that nickel chloride hexahydrate is not added.
[0110] The material obtained in this comparative example is used as a positive electrode catalyst for lithium oxygen batteries at 200mA g -1 Under the test conditions of current density and cutoff voltage of 2.35-4.35V, the specific capacity of the battery for the first charge / discharge is 10220.3 / 12885.2mAh g -1 , the coulombic efficiency is 79.3%; at a fixed specific capacity of 500mAh g -1 、Current density 600mAg -1 The charge / discharge test was carried out under the condition of 88 cycles; at the current density of 200mAg -1 , fixed specific capacity 600mAh g -1 The charge / discharge test was carried out under the test conditions and 59 cycle performances were obtained.
[0111] From the comparison between Example 1 and Comparative Examples 1-3, it can be seen that compared with RuO2 / Co3O4 nanosheets, RuO2 / NiO nanosheets or Co3O4 / NiO nanosheets, the electronic structure at the specific heterogeneous interface of RuO2 / Co3O4 / NiO porous nanosheets can better promote the transmission of electrons and enhance the coupling and synergistic effect between the various parts, significantly improving the specific capacity and cycle stability of the material.
[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst, characterized in that: include: Preparing a mixed solution of ruthenium salt, cobalt salt and nickel salt, wherein the molar ratio of ruthenium salt, cobalt salt and nickel salt is 10-30:40-80:10-50; RuO2 / Co3O4 / NiO porous nanosheets were prepared using a mixed solution of ruthenium salt, cobalt salt and nickel salt as raw materials and a glucose template method.
2. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 1, characterized in that: The specific steps of the glucose template method include: Glucose and urea are added to a mixed solution of ruthenium salt, cobalt salt and nickel salt, mixed evenly, and calcined to obtain the product.
3. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 1, characterized in that: The ruthenium salt is ruthenium trichloride hydrate; Or, the cobalt salt is cobalt chloride hexahydrate; Alternatively, the nickel salt is nickel chloride hexahydrate.
4. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 1, characterized in that: The molar ratio of urea to glucose is 3-5:5-7.
5. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 1, characterized in that: The calcination is performed under an air atmosphere.
6. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 1, characterized in that: The calcination was carried out in two steps.
7. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 6, characterized in that: The first calcination temperature is 120-160°C and the calcination time is 6-10h.
8. The method for preparing a high-performance RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 6, characterized in that: The second calcination temperature is 400-600°C and the calcination time is 10-14h.
9. A RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst prepared by the method according to any one of claims 1 to 8.
10. Use of the RuO2 / Co3O4 / NiO porous nanosheet lithium oxygen battery cathode catalyst according to claim 9 in preparing a cathode of a lithium oxygen battery or a lithium oxygen battery.
Citation Information
Cited By
Preparation method and application of two-dimensional Ru-Mn3O4 lithium-sulfur battery positive electrode catalyst
CN120961155A