Alkyl silyl peroxide, thermosetting composition, resin film, prepreg, metal laminate, and printed wiring board

By combining alkylsilyl peroxide with free radical polymerizable compounds, the problem of dialkyl peroxide decomposition too quickly at high temperatures is solved, and the sufficient curing reaction at high temperatures is achieved, and the material is improved. Heat resistance and dielectric properties.

CN119013284APending Publication Date: 2024-11-22NOF CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034246.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-27
Filing Date
2023-09-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing dialkyl peroxide decomposes too quickly at high temperatures, resulting in insufficient curing reaction of the thermosetting composition and the heat resistance and dielectric properties of the material cannot be ensured.

Method used

An alkyl silyl peroxide is used as a new polymerization initiator, combined with a radical polymerizable compound, and reacts it with a chlorosilane compound and a hydroperoxide through a preparation method to form a thermoset composition with a high decomposition temperature.

Benefits of technology

The decomposition temperature of the thermosetting composition is improved, the curing reaction at high temperature is ensured, the heat resistance and dielectric properties of the material are enhanced, the volatile components are reduced, and the performance of the cured substance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013284A_ABST
    Figure CN119013284A_ABST
Patent Text Reader

Abstract

The present invention provides an alkylsilyl peroxide which is one or more compounds selected from the group consisting of compounds represented by general formula (1) and compounds represented by general formula (2). The alkylsilyl peroxide is a novel polymerization initiator that can be used in a process for curing a thermally polymerizable composition at high temperatures. # imgabs0 # imgabs1 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an alkylsilyl peroxide, a thermosetting composition, a resin film, a prepreg, a metal laminate and a printed wiring board. Background Art

[0002] Organic peroxides decompose due to heat to generate free radicals, and can be used as polymerization initiators for plastics or crosslinking agents for rubbers. Organic peroxides can adjust the decomposition temperature by their chemical structure, and can be used at various processing temperatures from room temperature to about 200°C. Among these organic peroxides, dialkyl peroxides have a high decomposition temperature and can be used, for example, as a crosslinking agent for rubber. At this time, when kneading in a molten state of rubber at about 100°C, the rubber does not crosslink because the decomposition of dialkyl peroxide is very small. Free radicals can be generated by heating at about 180°C, and the rubber can be crosslinked.

[0003] On the other hand, with the remarkable progress of information network technology and the expansion of services that make full use of information networks, a kind of electronic equipment that can carry out large-capacity and high-speed processing speed of information is sought. Due to the popularization of the fifth-generation mobile communication system, this trend is further accelerated. Therefore, for electronic circuit substrate materials such as printed wiring boards for electronic equipment, while requiring excellent dielectric properties such as low dielectric constant and low dielectric loss tangent, high heat resistance is also required. With the high heat resistance of the material, the high temperature of the process temperature of the curing process is constantly advancing.

[0004] As a free radical polymerizable compound of a thermosetting composition used in an electronic circuit substrate material, polyphenylene ether or maleimide having a free radical polymerizable double bond at a molecular end is preferably used because of its excellent dielectric properties. In addition, a dialkyl peroxide can be used as the curing agent (Patent Documents 1 to 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2008 / 033612

[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-61409

[0009] Patent Document 3: International Publication No. 2020 / 158849 Summary of the invention

[0010] The alkyl peroxy radical generated by the decomposition of the dialkyl peroxide generates a carbon radical by secondary decomposition. The carbon radical is added to the double bond of the radical polymerizable compound to initiate a curing reaction. In addition, among dialkyl peroxides, the decomposition temperature of dialkyl peroxides is lower when the carbon chain is longer, such as tert-amyl or tert-hexyl, than when the carbon chain is shorter, such as tert-butyl. Therefore, the dialkyl peroxide with a longer carbon chain as described above decomposes too quickly in the curing process at a high temperature of more than 190°C, so the curing reaction cannot be fully carried out, and the heat resistance of the cured product cannot be fully ensured.

[0011] Therefore, the present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide an alkylsilyl peroxide as a novel polymerization initiator that can be used in a curing step of a heat-polymerizable composition at a high temperature.

[0012] (II) Technical solution

[0013] That is, the present invention relates to an alkylsilyl peroxide, wherein the alkylsilyl peroxide is one or more selected from the group consisting of a compound represented by the general formula (1) and a compound represented by the general formula (2),

[0014] [Chemical formula 1]

[0015]

[0016] In formula (1), R 1 and R 2 are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 3 is an alkyl group or a phenyl group having 3 to 6 carbon atoms, R 4 is an alkyl group having 2 to 5 carbon atoms,

[0017] [Chemical formula 2]

[0018]

[0019] In formula (2), R 5 and R 6 are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 7 is an alkyl group having 2 to 6 carbon atoms, R 8 It is ethylene or ethynylene.

[0020] Furthermore, the present invention relates to a thermosetting composition comprising the alkylsilyl peroxide and a radical polymerizable compound.

[0021] Furthermore, the present invention relates to a resin film formed of the thermosetting composition.

[0022] Furthermore, the present invention relates to a prepreg obtained by impregnating or coating a fibrous base material with the thermosetting composition.

[0023] Furthermore, the present invention relates to a metal-clad laminate including the resin film or the prepreg and a metal foil laminated together.

[0024] Furthermore, the present invention relates to a printed wiring board obtained by removing a portion of the metal foil from the metal-clad laminate.

[0025] Furthermore, the present invention relates to a method for preparing an alkylsilyl peroxide, which is a method for preparing the alkylsilyl peroxide, and the method comprises a step of using a chlorosilane compound and a hydroperoxide compound as raw materials and reacting them.

[0026] (III) Beneficial effects

[0027] Since the alkylsilyl peroxide of the present invention has a trialkylsilyl group, it has a higher decomposition temperature than a dialkyl peroxide, and can efficiently perform a curing step of a thermosetting composition at a high temperature.

[0028] In addition, in the case of a dialkyl peroxide such as di-tert-hexyl peroxide, there is a problem that a portion of the thermosetting composition volatilizes in the solvent drying step which is a pretreatment step of the curing step of the thermosetting composition. However, it is expected that an alkylsilyl peroxide having a trialkylsilyl group can suppress such volatilization.

[0029] In addition, since the above-mentioned thermosetting composition is suitable for curing at high temperature, the heat resistance of the obtained cured product can be improved. Furthermore, when a resin such as polyphenylene ether or maleimide is used as a free radical polymerizable compound contained in the thermosetting composition, since a low-polarity decomposition product such as an ethyl radical (carbon radical) can be introduced into the end of the resin, the dielectric properties of the cured product can be improved. DETAILED DESCRIPTION

[0030] <Alkylsilyl peroxide>

[0031] The alkylsilyl peroxide of the present invention is one or more selected from the group consisting of compounds represented by the general formula (1) and compounds represented by the general formula (2).

[0032] [Chemical formula 3]

[0033]

[0034] In formula (1), R 1 and R 2are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 3 is an alkyl group or a phenyl group having 3 to 6 carbon atoms, R 4 is an alkyl group having 2 to 5 carbon atoms,

[0035] [Chemical formula 4]

[0036]

[0037] In formula (2), R 5 and R 6 are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 7 is an alkyl group having 2 to 6 carbon atoms, R 8 It is ethylene or ethynylene.

[0038] In the formula (1), R 1 and R 2 For example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a phenyl group, etc. are mentioned.

[0039] In the formula (1), R 3 For example, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, phenyl, etc. can be mentioned.

[0040] In the formula (1), R 4 For example, an ethyl group, an n-propyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a neopentyl group, etc. are mentioned.

[0041] In the formula (2), R 5 and R 6 For example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a phenyl group, etc. are mentioned.

[0042] In the formula (2), R 7 For example, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, etc. are mentioned.

[0043] Specific examples of the alkylsilyl peroxide of the present invention are shown below, but the present invention is not limited to these examples.

[0044] [Chemical formula 5]

[0045]

[0046] As the dialkyl peroxide, preferably, Compound 1 to Compound 18 are listed, and more preferably, Compound 4, Compound 5, Compound 6, Compound 12, Compound 13, Compound 14, Compound 16, and Compound 19 are listed. As the dialkyl peroxide, more preferably, one of the substituents of the silyl group is a tert-butyl group and the other two substituents are methyl groups, all the substituents of the silyl group are phenyl groups, one of the substituents of the silyl group is a phenyl group and the other two substituents are methyl groups, or two of the substituents of the silyl group are phenyl groups and the other one substituent is methyl groups.

[0047] <Method for preparing alkylsilyl peroxide>

[0048] The method for producing the alkylsilyl peroxide represented by the general formula (1) is not limited in any way, and examples thereof include a method comprising a step of reacting a hydroperoxide represented by the general formula (3) with a chlorosilane compound represented by the general formula (4) (hereinafter also referred to as step (X)).

[0049] [Chemical formula 6]

[0050]

[0051] [Chemical formula 7]

[0052]

[0053] The method for producing the alkylsilyl peroxide represented by the general formula (2) is not limited in any way, and examples thereof include a method comprising a step (hereinafter also referred to as step (Y)) of reacting a hydroperoxide compound represented by the general formula (5) with a chlorosilane compound represented by the general formula (4).

[0054] [Chemical formula 8]

[0055]

[0056] In the step (X) or the step (Y), commercially available products can be used as the hydroperoxide compound represented by the general formula (3) or (5) and the chlorosilane compound represented by the general formula (4).

[0057] In the step (X), from the perspective of improving the yield of the target product, it is preferred to use 0.8 to 5.0 moles of the hydroperoxide compound represented by the general formula (3) relative to 1.0 mole of the chlorosilane compound represented by the general formula (4), and it is further preferred to use 1.0 to 3.0 moles. In addition, in the step (Y), from the perspective of improving the yield of the target product, it is preferred to use 0.4 to 10.0 moles of the hydroperoxide compound represented by the general formula (5) relative to 1.0 mole of the chlorosilane compound represented by the general formula (4), and it is further preferred to use 0.5 to 6.0 moles.

[0058] In the step (X) or the step (Y), it is preferred to use a base catalyst. The base catalyst is not particularly limited, and examples thereof include pyridine, dimethylaminopyridine, triethylamine, sodium hydroxide, potassium hydroxide, sodium carbonate, etc. The base catalyst may be used alone or in combination of two or more.

[0059] In the step (X) or the step (Y), the amount of the base catalyst used is not particularly limited. From the perspective of improving the yield of the target product, it is preferred to use 0.1 mol to 5.0 mol of the base catalyst relative to 1.0 mol of the chlorosilane compound represented by the general formula (4), and it is further preferred to use 1.0 mol to 3.0 mol.

[0060] In the step (X) or the step (Y), an organic solvent is preferably used. The organic solvent is not particularly limited, and is preferably an inactive organic solvent in the reaction system. Examples of the organic solvent include non-polar compounds such as pentane, hexane, and toluene; polar compounds such as acetone, acetonitrile, tetrahydrofuran, and vinyl acetate. The organic solvent may be used alone or in combination of two or more.

[0061] In the step (X) or the step (Y), the amount of the organic solvent used is not particularly limited, and is usually about 0.1 to 100 parts by mass relative to 1 part by mass of the chloride represented by the general formula (4) or the general formula (6).

[0062] From the perspective of improving the yield of the target product, the reaction temperature of the step (X) or the step (Y) is preferably above -10°C, more preferably above 0°C, and from the perspective of safety, it is preferably below 60°C, more preferably below 50°C.

[0063] The reaction time of the step (X) or the step (Y) varies depending on the raw materials, reaction temperature, etc. and therefore cannot be determined in general. However, from the perspective of improving the yield of the target product, the reaction time is generally preferably 0.1 hours or more, more preferably 0.5 hours or more, and preferably 5 hours or less.

[0064] The step (X) or the step (Y) may be performed in an air atmosphere at normal pressure, or may be performed in a nitrogen atmosphere or a nitrogen gas stream.

[0065] After the step (X) or the step (Y), in order to remove excess raw materials or by-products, the alkylsilyl peroxide can be purified by washing with an aqueous electrolyte solution such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium sulfite, hydrogen chloride, sulfuric acid, sodium chloride, or ion exchange water.

[0066] The obtained alkylsilyl peroxide can be identified by gas chromatography (GC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), infrared spectroscopy (IR), mass spectrometry (MS) or the like.

[0067] <Thermosetting composition>

[0068] The thermosetting composition of the present invention contains an alkylsilyl peroxide and a radical polymerizable compound. In addition, the thermosetting composition may contain other components in combination as appropriate.

[0069] <Radical polymerizable compounds>

[0070] As long as it can be polymerized by a thermal free radical polymerization reaction, there is no particular limitation on the free radical polymerizable compound, and examples thereof include compounds having ethylenically unsaturated groups such as a vinyl group, an allyl group, a methacryloyl group, a styryl group, a methyl (acrylic) group, and a maleimide group. From the perspective of being able to use the above-mentioned alkyl silyl peroxide to improve the dielectric properties and heat resistance of the cured product, examples thereof include polyphenylene ether and maleimide.

[0071] The polyphenylene ether is not particularly limited as long as it has a radical polymerizable double bond at a molecular terminal. The polyphenylene ether having a radical polymerizable double bond may be used alone or in combination of two or more.

[0072] Specific examples of the structural unit of the polyphenylene ether include poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), etc. From the viewpoint of excellent dielectric properties and heat resistance, poly(2,6-dimethyl-1,4-phenylene ether) is preferred. Furthermore, specific examples of the structural unit of the polyphenylene ether include: copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, 2-allylphenol, etc.); polyphenylene ether copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols; and polyphenylene ethers having a linear or branched structure obtained by heating poly(2,6-dimethyl-1,4-phenylene ether) and a phenol compound such as bisphenols or triphenols in a toluene solvent in the presence of an organic peroxide to perform a redistribution reaction. The phenylene group in the phenylene ether unit may have a substituent, and the polyphenylene ether may contain other structural units other than the phenylene ether unit within the range that does not hinder the effect of the present invention.

[0073] Examples of the radical polymerizable double bond at the molecular end include (meth)acryloyl, styryl, vinylbenzyl, vinyl, allyl, 1,3-butadienyl, etc. Among these groups, (meth)acryloyl and vinylbenzyl are preferred because of their high reactivity during thermal curing and excellent dielectric constant or dielectric loss tangent of the cured product.

[0074] The number of radically polymerizable double bonds in one molecule of the polyphenylene ether having radically polymerizable double bonds at the molecular terminals is preferably 1.5 to 6 on average, more preferably 1.6 to 4 on average, and even more preferably 1.7 to 3 on average.

[0075] The number of ethylenically unsaturated double bonds in one molecule of the polyphenylene ether having a free radical polymerizable double bond at the molecular end can be measured, for example, by measuring the number of hydroxyl groups remaining in the polyphenylene ether and calculating the portion of the hydroxyl group number reduced compared to the polyphenylene ether before modification with the compound having ethylenically unsaturated double bonds. In addition, the method for measuring the number of hydroxyl groups remaining in the polyphenylene ether can be obtained by the following method: according to the method described in Polymer Thesis Collection, Vol. 51, No. 7, p. 480 (1994), tetraethylammonium hydroxide is added to a dichloromethane solution of the polyphenylene ether and the absorbance of the mixed solution at a wavelength of 318 nm is measured.

[0076] Furthermore, the polyphenylene ether having a radical polymerizable double bond at a molecular terminal preferably has a structure represented by the following general formula (6).

[0077] [Chemical formula 9]

[0078]

[0079] In formula (6), X is an arbitrary linking group having a valence of a, Y is a radical polymerizable double bond at the molecular terminal, and a is 1 to 6.

[0080] In the formula (6), specific examples of X include divalent phenols such as bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 4,4'-dihydroxy-3,3'5,5'-tetramethylbiphenyl, 4,4'-dihydroxy-2,2',3,3',5,5'-hexamethylbiphenyl, hydroquinone, and resorcinol; and trivalent or higher phenols such as tris(4-hydroxyphenyl)methane, 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, phenol novolac, o-cresol novolac, and naphthol novolac.

[0081] From the viewpoint of dielectric properties and permeability into a fibrous substrate, the number average molecular weight of the polyphenylene ether having a radically polymerizable double bond at a molecular terminal is preferably 800 to 5000, more preferably 900 to 4500, and even more preferably 1000 to 3000.

[0082] The number average molecular weight can be a value obtained by measuring using a common molecular weight measuring method, and examples thereof include a polystyrene conversion value obtained by measuring using gel permeation chromatography (GPC), etc. Specifically, after preparing a measurement sample having a sample concentration of 0.2 w / vol% (solvent: chloroform), HLC-8220GPC (manufactured by TOSOH CORPORATION) can be used as a measuring device, and the measurement is performed under the conditions of a chromatographic column: Shodex GPC KF-405L HQ×3 (manufactured by Showa Denko KK), an eluent: chloroform, an injection volume: 20 μL, a flow rate: 0.3 mL / min, a chromatographic column temperature: 40° C., and a detector: RI.

[0083] The synthesis method of the polyphenylene ether having a free radical polymerizable double bond at the molecular end is not particularly limited as long as it is possible to synthesize a modified polyphenylene ether modified using a free radical polymerizable double bond. Specifically, a method of reacting a compound having an ethylenically unsaturated double bond and a chlorine atom with a polyphenylene ether before modification, etc. can be cited. As a compound having an ethylenically unsaturated double bond and a chlorine atom, for example, (meth)acryloyl chloride or vinylbenzyl chloride can be cited. In addition, the polyphenylene ether having a free radical polymerizable double bond at the molecular end can use a commercial product, for example, the product name "OPE-2St" (manufactured by Mitsubishi Gas Chemical Company, Inc.), "Noryl SA9000" (manufactured by SABIC Innovative Plastics Co., Ltd.), etc. can be cited.

[0084] The maleimide is not particularly limited as long as it is a compound having a maleimide group in the molecule. As the maleimide, a monofunctional maleimide having one maleimide group in the molecule and a polyfunctional maleimide having two or more maleimide groups in the molecule can be listed. The maleimide can be used alone or in combination of two or more.

[0085] Specific examples of the maleimide include, for example, the monofunctional maleimide, phenylmaleimide, cyclohexylmaleimide, chlorophenylmaleimide such as o-chlorophenylmaleimide, methylphenylmaleimide such as o-methylphenylmaleimide, hydroxyphenylmaleimide such as p-hydroxyphenylmaleimide, carboxyphenylmaleimide such as p-carboxyphenylmaleimide, N-dodecylmaleimide, and phenylmethanemaleimide. Examples of the polyfunctional maleimide include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, phenylene bismaleimide such as m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, and 1,3-bis(4-maleimidophenoxy)benzene. Among these maleimides, polyfunctional maleimides are preferred from the viewpoint of the glass transition temperature of the cured product, and 4,4′-diphenylmethanebismaleimide and 3,3′-dimethyl-5,5′-diethyl-4,4′-diphenylmethanebismaleimide are more preferred.

[0086] The maleimide may be a commercially available product, for example, product names "BMI-1000", "BMI-4000", and "BMI-5100" manufactured by DAIWA KASEI INDUSTRIAL Co., Ltd., product names "BMI-689", "BMI-2560", "BMI-3000", and "BMI-5000P" manufactured by DESIGNER MOLECULES, INC., and product name "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.

[0087] The dialkyl peroxide may be used in any amount relative to the radical polymerizable compound, and is usually used in an amount of preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the radical polymerizable compound.

[0088] <Other ingredients>

[0089] The thermosetting composition of the present invention can further contain other components in appropriate combination. Other components include polyfunctional monomers, solvents, organic peroxides, azo compounds, polyisoprene, polybutadiene, styrene butadiene rubber, butyl rubber, ethylene propylene rubber, ethylene-propylene-diene rubber, styrene-butadiene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, ethylene-styrene-divinylbenzene copolymer, ethylene-hexene-styrene-divinylbenzene copolymer, fluororubber, silicone rubber and other elastomers, natural silica, molten silica, etc. Silica, synthetic silica, amorphous silica, hollow silica, alumina, boron nitride, aluminum nitride, clay, talc and glass short fiber and other inorganic fillers, γ-aminopropyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-(meth)acryloxypropyl trimethoxysilane and other silane coupling agents, flame retardants, polymerization inhibitors, ultraviolet absorbers, light stabilizers, metal passivators, surfactants, lubricants, thickeners, defoamers, antistatic agents, pigments, dyes, etc.

[0090] From the perspective of adjusting the viscosity of the thermosetting composition or improving the heat resistance of the cured product, the multifunctional monomer can be blended. As the multifunctional monomer, for example, multifunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-divinylbenzene, vinylbenzene derivatives such as 4-vinylbenzoic acid-2-acryloylethyl ester, alkenyl isocyanurate derivatives such as triallyl isocyanurate (TAIC), alkenyl cyanurate derivatives such as triallyl cyanurate (TAC), etc. can be listed. Among these multifunctional monomers, triallyl isocyanurate and triallyl cyanurate are preferred due to their excellent heat resistance. The multifunctional monomer can be used alone or in combination of two or more.

[0091] The amount of the polyfunctional monomer is preferably 5 to 50 parts by mass, more preferably 7 to 40 parts by mass, and even more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the radical polymerizable compound.

[0092] The solvent may be added from the viewpoint of improving the viscosity of the thermosetting composition, the permeability to glass cloth, the smoothness of the cured film, etc. The solvent is not particularly limited as long as it can dissolve or disperse the above-mentioned components and volatilizes during drying.

[0093] From the perspective of solubility, the solvent is preferably an aromatic solvent such as toluene and xylene; a ketone solvent such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone; an amide solvent such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone. These solvents can be used alone or in combination of two or more. From the perspective of the solubility of the thermosetting composition in the solvent and the ease of the volatilization process, the amount of the solvent used is preferably 10 to 1000 parts by mass, and more preferably 20 to 500 parts by mass, relative to 100 parts by mass of the solid content of the thermosetting composition.

[0094] <Method for preparing thermosetting composition>

[0095] When preparing the thermosetting composition, the alkylsilyl peroxide and the radical polymerizable compound are added to the storage container and other components are added as needed, and a ball mill, a bead mill, a planetary mixer, a roller mill, etc. are used to dissolve or disperse according to a conventional method. At this time, heating can be performed as needed. When the radical polymerizable compound is dissolved in the solvent by heating, unnecessary gelation can be suppressed by cooling to 50° C. or less after dissolution and then blending the alkylsilyl peroxide. In addition, filtering can be performed through a sieve or a membrane filter as needed.

[0096] <Resin film>

[0097] The resin film of the present invention is formed from the thermosetting composition. The resin film contains the thermosetting composition before curing, but a part of the thermosetting composition may be cured. The resin film can be obtained, for example, by drying a resin varnish which is a mixture of the thermosetting composition and the solvent alone, or by coating the resin varnish on a support such as a support film and then drying it. The solvent can be dried and removed using a hot air dryer, for example, at 20°C to 180°C. The drying temperature is preferably 20 to 150°C, more preferably 50 to 130°C.

[0098] Examples of the support of the resin film include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polycarbonate, polyimide, ethylene-tetrafluoroethylene copolymers, metal foils such as copper foil and aluminum foil, and release paper. A metal foil obtained by coating the thermosetting composition on a metal foil and then drying and removing the solvent using a hot air dryer is referred to as a metal foil with resin. In addition, the support may be subjected to chemical or physical treatments such as matte treatment, corona treatment, and release treatment.

[0099] The resin film is suitable as an interlayer insulating sheet, an adhesive film, or the like of a laminate such as a multilayer printed wiring board.

[0100] <Prepreg>

[0101] The prepreg of the present invention is a composite of a fibrous substrate and the thermosetting composition. The prepreg contains a thermosetting composition before curing, but a part of the thermosetting composition can be cured. The prepreg is preferably a composite of a fibrous substrate and a thermosetting composition impregnated or coated on the fibrous substrate. Even when the thermosetting composition is applied to the surface of the fibrous substrate and a layer is formed, a structure in which a cured product of the thermosetting composition is impregnated in the substrate can be obtained by compression molding for curing the prepreg. The prepreg can be obtained, for example, by the following method: a resin varnish which is a mixture of the thermosetting composition of the present invention and a solvent is impregnated or coated on a substrate such as glass cloth, and then the solvent is dried to remove. In addition, the impregnation or coating can be repeated multiple times. Furthermore, it is also possible to adjust to the desired impregnation amount by using a plurality of thermosetting compositions with different concentrations or compositions for repeated impregnation or coating. The drying and removal of the solvent uses a hot air dryer, for example, at 20°C to 180°C. The drying temperature is preferably 20 to 150°C, more preferably 50 to 130°C.

[0102] As the fibrous substrate, for example, glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, pulp paper and cotton linter paper can be cited. Among them, glass cloth is preferred because the mechanical strength of the printed wiring board is excellent, and glass cloth processed by flattening is more preferred. These fibrous substrates can be used alone or in combination of two or more. In addition, as the thickness of the fibrous substrate, for example, a fibrous substrate of 1 to 300 μm can be used.

[0103] In the solid content of the prepreg, the ratio of the solid content of the thermosetting composition is preferably 30 to 80% by mass, more preferably 40 to 70% by mass. When the above ratio is less than 30% by mass, there is a tendency for poor insulation reliability when the prepreg is used for electronic substrates, etc. In addition, when the above ratio is more than 80% by mass, there is a tendency for poor mechanical properties such as bending elastic modulus when used for electronic substrates, etc.

[0104] <Metal-clad laminate>

[0105] The metal-clad laminate of the present invention is a laminate formed by laminating the resin film or the prepreg with a metal foil. The laminate can be manufactured by overlapping one or more sheets of the resin film and / or prepreg with a substrate such as a metal foil, and then curing the thermosetting composition by compression molding to form an insulating layer. The metal foil with the resin can also be used instead of the metal foil. The heat molding can be performed, for example, at a temperature of 180°C to 240°C, a heating time of 30 minutes to 300 minutes, and a pressure of 20 kgf / cm 2 ~40kgf / cm 2 The surface pressure is carried out.

[0106] The metal foil is not particularly limited, and examples thereof include aluminum foil and copper foil, and among them, copper foil is preferred because of its low electrical resistance. As the thickness of the metal foil, for example, a metal foil of 1 to 50 μm can be used.

[0107] The resin film and prepreg combined with the metal foil may be one sheet or multiple sheets, and the metal foil may be laminated on one or both sides to form a laminate depending on the application. The metal-clad laminate is particularly suitable as a printed wiring board.

[0108] <Printed wiring board>

[0109] The printed wiring board of the present invention can be obtained by removing a portion of the metal foil on the surface of the metal-clad laminate by etching or the like to form wiring, thereby forming a circuit on the surface of a resin film or a prepreg. Since the printed wiring board contains the thermosetting composition, the dielectric constant or dielectric loss tangent and other dielectric properties, moldability, and heat resistance are excellent.

[0110] In addition to the above, the thermosetting composition can also be used for molding, lamination, adhesives, copper-clad laminates and other composite materials. In particular, when isocyanate or epoxy is used alone or in combination, representative examples of applications include prepregs formed by semi-curing resins and laminates formed by curing the prepregs. In addition, when epoxy is used, representative examples of applications in semiconductor sealing materials can be cited.

[0111] Example

[0112] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following examples at all.

[0113] <Synthesis of alkylsilyl peroxide>

[0114] <Preparation Example 1, Synthesis of Compound 5>

[0115] In a 500 mL round-bottom flask, tert-butyldimethylsilyl chloride (purity 99%, 90.43 g, 0.6 mol), toluene (74.50 g), and tert-hexyl hydroperoxide (purity 85.0%, 74.45 g, 0.63 mol) were added and stirred. The above solution was cooled to 15°C, and pyridine (purity 99%, 94.42 g, 1.20 mol) was added dropwise. After the addition was completed, the mixture was stirred for 1 hour, and the obtained solution was reduced and cleaned with an aqueous sodium sulfite solution, and then washed with water. Then, sodium sulfate and magnesium sulfate were used for dehydration to obtain R of the above general formula (1): 1 and R 2 Represents methyl, R 3 Represents tert-butyl, R 4 A toluene solution of tert-butyldimethyl(tert-hexylperoxy)silane representing a propyl group (203.4 g, concentration 24.2% by mass, yield 35.3% by mass).

[0116] In addition, the AVANCE N NMR spectrometer (manufactured by Bruker Corporation) was used. 1 H-NMR measurement, 13 The structure of the alkylsilyl peroxide was identified by C-NMR measurement and TOFMS (manufactured by JEOL LTD.). In addition, the purity was calculated by the simple area method in GC (GC-2014 series manufactured by Shimadzu Corporation). The obtained compound 5 was purified by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0117] <Preparation Example 2, Synthesis of Compound 6>

[0118] The preparation was the same except that tert-hexyl hydroperoxide in Preparation Example 1 was replaced with 1,1,3,3-tetramethylbutyl hydroperoxide. A toluene solution of tert-butyldimethyl(1,3,3-tetramethylbutylperoxy)silane (186.46 g, concentration 31.3 mass %, yield 37.3 mass %) was obtained. The obtained compound 6 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0119] <Preparation Example 3, Synthesis of Compound 4>

[0120] Except that the tert-hexyl hydroperoxide in Preparation Example 1 was changed to tert-amyl hydroperoxide, the other procedures were the same. A toluene solution of tert-butyldimethyl (tert-amylperoxy) silane (185.35 g, concentration 25.2 mass %, yield 35.7 mass %) was obtained. The obtained compound 4 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0121] <Preparation Example 4, Synthesis of Compound 13>

[0122] The same procedures were followed except that the tert-butyldimethylsilyl chloride in Preparation Example 1 was replaced with triphenylsilyl chloride. A toluene solution of triphenyl(tert-hexylperoxy)silane (328.1 g, concentration 24.3% by mass, yield 70.5% by mass) was obtained. The obtained compound 13 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0123] <Preparation Example 5, Synthesis of Compound 14>

[0124] The preparation was the same except that the tert-butyldimethylsilyl chloride in Preparation Example 1 was changed to triphenylsilyl chloride and the tert-hexyl hydroperoxide was changed to 1,1,3,3-tetramethylbutyl hydroperoxide. A toluene solution of triphenyl(1,3,3-tetramethylbutylperoxy)silane (386.3 g, concentration 24.0 mass %, yield 76.3 mass %) was obtained. The obtained compound 14 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0125] <Preparation Example 6, Synthesis of Compound 12>

[0126] Except that the tert-butyldimethylchlorosilane in Preparation Example 1 was changed to triphenylchlorosilane and the tert-hexyl hydroperoxide was changed to tert-amyl hydroperoxide, the other procedures were the same. A toluene solution of triphenyl (tert-amyl peroxy) silane (316.1 g, concentration 23.6 mass %, yield 68.5 mass %) was obtained. The obtained compound 12 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0127] <Preparation Example 7, Synthesis of Compound 16>

[0128] Dimethylaminopyridine (purity 99%, 122.17 g, 1.0 mol), tetrahydrofuran (201.35 g), 2,5-dimethyl-2,5-di-tert-butyl hydroperoxide (purity 75.5%, 62.56 g, 0.27 mol) were added to a 500 mL round-bottom flask and stirred. The above solution was cooled to 15°C, and a solution of tert-butyldimethylchlorosilane (purity 99%, 90.43 g, 0.6 mol) in tetrahydrofuran (30.0 g) was added dropwise. After the addition was completed, the mixture was stirred for 3 hours, and the obtained solution was reduced and washed with an aqueous sodium sulfite solution, and then washed with water. Then, sodium sulfate and magnesium sulfate were used for dehydration to obtain R of the above general formula (2): 5 and R 6 Represents methyl, R 7 Represents tert-butyl, R 8 Representing ethylene 2,2,3,3,6,6,9,9,12,12,13,13-dodecyl-4,5,10,11-tetraoxa-3,12-disila tetradecane toluene solution. Then, silica gel column chromatography was used to separate and obtain 2,2,3,3,6,6,9,9,12,12,13,13-dodecyl-4,5,10,11-tetraoxa-3,12-disila tetradecane (44.5 g, purity 99.9%, yield 21.9% by mass). The obtained compound 16 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0129] <Preparation Example 8, Synthesis of Compound 19>

[0130] The same procedures were followed except that the tert-butyldimethylchlorosilane in Preparation Example 1 was replaced with phenyldimethylchlorosilane. A toluene solution of phenyldimethyl (tert-hexylperoxy) silane (220.4 g, concentration 58.8% by mass, yield 70.2% by mass) was obtained. The obtained compound 19 was analyzed by EI-MS and 1 The analysis results obtained by H-NMR are shown in Table 1.

[0131] <Evaluation of decomposition starting temperature>

[0132] As DSC (differential scanning calorimeter), "DSC-7000X" manufactured by Hitachi High-Tech Science Corporation was used. During the measurement, about 8 mg of the synthetic sample was placed in a stainless steel box, and the temperature was raised from 50°C to 300°C at a rate of 10°C per minute under a nitrogen atmosphere. In addition, the decomposition starting temperature was set to the intersection of the initial baseline of the DSC and the tangent at the inflection point of the curve. The measurement results of the decomposition starting temperature (°C) of the dialkyl peroxides synthesized in Preparation Examples 1 to 7 are shown in Table 1. In addition, as reference examples for comparison of Preparation Examples 1 to 7, the results of di-tert-butyl peroxide, di-tert-hexyl peroxide, and 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane are shown.

[0133] [Table 1]

[0134]

[0135] Since the alkylsilyl peroxide of the preparation example has a high decomposition temperature, the curing step of the thermosetting composition at a high temperature can be efficiently carried out.

[0136] <Evaluation of volatility>

[0137] The weight reduction rate (%) of the dialkyl peroxide synthesized in Preparation Examples 5 and 7 was measured using TG-DTA6200 manufactured by SII NanoTechnology Inc. (measurement conditions: aluminum box, air atmosphere, temperature rise 30°C (90°C / min) → 80°C (30 minutes), sample amount 15 mg). The results are shown in Table 2.

[0138] [Table 2]

[0139]

[0140] <Examples 1 to 13, Comparative Examples 1 to 6>

[0141] <Preparation of cured products and evaluation of dielectric properties>

[0142] Each component (parts by mass) shown in Tables 3 and 4 was diluted with toluene and blended in a concentration of 50% by mass, and 6 g of the solvent solution of the composition thus obtained was placed in an aluminum dish, and a vacuum dryer (EYELA VACUUMOVEN VOS-3LSD) was used to dry at 400 Pa and 60 ° C for 2 hours, and then the solvent was further dried at 80 ° C for 2 hours. A hand press (manufactured by TOYOSEIKI Co., Ltd.) was used to mold the obtained powder at 130 ° C and solidify it at 200 ° C to obtain a solidified product (film, 16 cm round, 60 μm thick). The dielectric constant and dielectric loss tangent of the obtained solidified product at 1 GHz were measured using a method based on IPC-TM-650-2.5.5.9, and are shown in Tables 3 and 4.

[0143] <Evaluation of heat resistance>

[0144] As a DSC (differential scanning calorimeter), a "DSC-7000X" manufactured by Hitachi High-Tech Science Corporation was used to measure the glass transition temperature of the above-mentioned cured product. During the measurement, a synthetic sample of about 2 mg was placed in an aluminum box, and the temperature was raised from 50°C to 350°C under a nitrogen atmosphere at a heating rate of 10°C per minute. In addition, the glass transition temperature was set to the temperature at the point where the straight line, which is equal in the longitudinal direction to the straight line extending from the low temperature side baseline and the straight line extending from the high temperature side baseline, intersected with the curve of the step-shaped change portion of the glass transition. The results are shown in Tables 3 and 4.

[0145] [Table 3]

[0146]

[0147] [Table 4]

[0148]

[0149] In Tables 3 and 4, OPE-2St 2200 represents a polyphenylene ether having an average of two ethylenically unsaturated double bonds at the molecular ends (number average molecular weight of 2200), manufactured by Mitsubishi Gas Chemical Company, Inc.;

[0150] OPE-2St 1200 represents a polyphenylene ether having an average of 2 ethylenically unsaturated double bonds at the molecular ends (number average molecular weight 1200), manufactured by Mitsubishi Gas Chemical Company, Inc.;

[0151] SA9000 indicates a polyphenylene ether having an average of 2 ethylenically unsaturated double bonds at the molecular ends (number average molecular weight 2756), manufactured by SABIC Innovative Plastics;

[0152] BMI-1000 stands for maleimide, manufactured by Tokyo Chemical Industry Co., Ltd.;

[0153] BMI-5100 represents maleimide, manufactured by Tokyo Chemical Industry Co., Ltd.;

[0154] Compound 5 represents tert-butyldimethyl(tert-hexylperoxy)silane of Preparation Example 1 (concentration 24.2 mass %);

[0155] Compound 6 represents tert-butyldimethyl(1,3,3-tetramethylbutylperoxy)silane (concentration 31.3 mass %) of Preparation Example 2;

[0156] Compound 4 represents tert-butyldimethyl(tert-amylperoxy)silane of Preparation Example 3 (concentration 25.2 mass %);

[0157] Compound 13 represents triphenyl(tert-hexylperoxy)silane of Preparation Example 4 (concentration 24.3 mass %);

[0158] Compound 14 represents triphenyl(1,3,3-tetramethylbutylperoxy)silane (concentration: 24.0 mass %) of Preparation Example 5;

[0159] Compound 12 represents triphenyl(tert-amylperoxy)silane of Preparation Example 6 (concentration 23.6 mass %);

[0160] Compound 16 represents 2,2,3,3,6,6,9,9,12,12,13,13-dodecamethyl-4,5,10,11-tetraoxa-3,12-disilatetradecane of Preparation Example 7;

[0161] Compound 19 represents phenyldimethyl(tert-hexylperoxy)silane of Preparation Example 8 (concentration 58.8 mass %);

[0162] Di-tert-butyl peroxide was manufactured by NOF Corporation (purity 98%);

[0163] Di-tert-hexyl peroxide was manufactured by NOF Corporation (purity 90%);

[0164] 2,5-Dimethyl-2,5-(di-tert-butylperoxy)hexane was manufactured by NOF Corporation (purity 94%);

[0165] TAIC (Triallyl Isocyanurate) was manufactured by Tokyo Chemical Industry Co., Ltd. (purity: 96.0%).

[0166] Compared with Comparative Examples 1 to 5, Examples 1 to 11 can obtain cured products having excellent physical properties, and compared with Comparative Examples 6 to 7, Examples 12 to 13 can obtain cured products having excellent physical properties.

Claims

1. An alkylsilyl peroxide, characterized in that The alkylsilyl peroxide is one or more selected from the group consisting of compounds represented by general formula (1) and compounds represented by general formula (2), [Chemical formula 1] In formula (1), R 1 and R 2 are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 3 is an alkyl group or a phenyl group having 3 to 6 carbon atoms, R 4 is an alkyl group having 2 to 5 carbon atoms, [Chemical formula 2] In formula (2), R 5 and R 6 are independently an alkyl group having 1 to 6 carbon atoms or a phenyl group, R 7 is an alkyl group having 2 to 6 carbon atoms, R 8 It is ethylene or ethynylene.

2. A thermosetting composition, characterized in that: The thermosetting composition contains the alkylsilyl peroxide according to claim 1 and a radical polymerizable compound.

3. The thermosetting composition according to claim 2, characterized in that The free radical polymerizable compound is polyphenylene ether or maleimide.

4. A resin film, characterized in that The resin film is formed from the thermosetting composition according to claim 3.

5. A prepreg, characterized in that: The thermosetting composition according to claim 3 is impregnated or coated on a fibrous substrate.

6. A metal-clad laminate, characterized in that: The metal-clad laminate is formed by laminating the resin film according to claim 4 or the prepreg according to claim 5 and a metal foil.

7. A printed wiring board, characterized in that It is obtained by removing part of the metal foil from the metal-clad laminate according to claim 6.