Fluorinated modified MOF glass film as well as preparation method and application thereof
By introducing fluorine elements into the MOF film to form a fluorinated modified MOF glass film, the problems of complex preparation of existing MOF glass films and poor separation stability under high humidity environments are solved, and high selective gas separation and stability improvement are achieved. Simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202411191137.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing MOF glass film preparation method is complex and not suitable for gas separation, and has poor separation stability under high humidity environments.
Using fluorinated modified MOF glass film, amorphous MOF glass structure is formed by introducing fluorine elements into the MOF film, increasing pore size selectivity, and heating fluorine-containing steam to contact the MOF film to form fluorine-containing steam Modified MOF glass film to improve hydrophobic performance.
Highly selective gas separation is achieved, separation stability is improved in high humidity environments, and the preparation process is simplified and costs are reduced.
Smart Images

Figure CN119015912A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of membrane materials, and in particular to a fluorinated MOF glass membrane and a preparation method and application thereof. Background Art
[0002] Membrane separation has the advantages of high energy efficiency, low operating cost, small footprint, and continuous operation. Compared with traditional separation methods with high energy consumption, membrane separation is very promising for gas separation. MOF is a new type of nanoporous organic-inorganic hybrid with a regular lattice with a rigid pore structure. MOF is composed of metal nodes and multi-toothed organic connectors interconnected to produce different structures and chemical functions, with clear pores, channels and cavities at the molecular scale. MOF glass material is a newly developed MOF material. MOF glass membrane has the advantages of no intercrystalline defects, permanent porosity and easy processing. Moreover, MOF glass has structural diversity and structural adjustability, which is impossible for traditional inorganic and organic glasses. At present, the preparation method of MOF glass membrane is mainly prepared by melt quenching method, in which polycrystalline membrane is melted at high temperature to become glass membrane, but this method requires multiple steps such as preparation of polycrystalline membrane and high-temperature melting in a tubular furnace. It is very meaningful if a MOF glass membrane with high performance can be obtained by a simple method. Summary of the invention
[0003] The object of the present invention is to provide a MOF membrane with high selectivity and simple preparation method. In order to achieve the above object, the first aspect of the present invention provides a fluorinated modified MOF glass membrane, in which organic ligands and fluorine ligands are present, wherein the molar ratio of the organic ligands to the fluorine ligands is (25~80):(20~75).
[0004] Preferably, the organic ligand is selected from any one or more of imidazole-2-carboxaldehyde, 2-methylimidazole, benzimidazole, 2-aminobenzimidazole, 4,5-dichloroimidazole, 2-nitroimidazole, 4-methylimidazole-5-carboxaldehyde.
[0005] Preferably, the metal element framework of the fluorinated modified MOF glass membrane is zinc element and / or cobalt element.
[0006] Compared with the prior art, the fluorinated MOF glass membrane provided by the present invention has the following beneficial effects: the present invention is modified on the basis of the existing metal organic skeleton membrane. Unlike the metal organic skeleton membrane in the prior art, the fluorinated MOF glass membrane provided by the present invention is an amorphous MOF glass structure. Since the fluorine element is introduced into the MOF membrane, the pore size of the fluorinated MOF glass membrane provided by the present invention is smaller, and it has higher selectivity in gas separation. At the same time, because the present invention introduces the fluorine element into the MOF membrane, the hydrophobicity of the membrane is greatly improved, and the water contact angle is greatly increased, which greatly improves the separation stability of the MOF membrane in a high humidity environment.
[0007] Furthermore, the second aspect of the present invention provides a method for preparing the fluorinated modified MOF glass film according to the first aspect, comprising the following steps:
[0008] S1: Preparation of MOF membrane;
[0009] S2: heating the fluorine-containing imidazole ligand to generate fluorine-containing vapor, which contacts the MOF membrane to form a MOF-F glass membrane;
[0010] S3: activating the MOF-F glass film in an activator to obtain a fluorinated modified MOF glass film.
[0011] Preferably, in step S1, the carrier used to prepare the MOF membrane is selected from one of α-Al2O3 carrier, γ-Al2O3 carrier, anodized aluminum carrier, TiO2 carrier, PVDF carrier, PAN carrier, PES carrier, PTFE carrier and PEI carrier.
[0012] Preferably, in step S2, the fluorine-containing ligand is selected from any one or more of monofluoromethylimidazole, difluoromethylimidazole, trifluoromethylimidazole, and 2-methyl-4-fluoroimidazole.
[0013] Preferably, in step S2, the heating temperature for heating the fluorine-containing imidazole ligand to generate fluorine-containing steam is 60-100°C.
[0014] Preferably, in step S2, the contact time between the fluorine-containing steam and the MOF membrane is 6 to 48 hours.
[0015] Preferably, in step S3, the activating agent is selected from any one or more of dichloromethane, chloroform, dimethylformamide, methanol, ethanol, chloroform, acetone, acetonitrile, chloroform, acetone, and dimethylformamide.
[0016] Preferably, in step S3, the activation time is 0.5 to 24 hours.
[0017] The preparation method of the fluorinated modified MOF glass film provided by the present invention has the advantage of simple processing technology, and the fluorinated imidazole ligand therein can be used multiple times, which has the advantage of high economy and practicability.
[0018] Furthermore, the third aspect of the present invention provides an application of the fluorinated modified MOF glass membrane described in the first aspect, specifically separating the fluorinated modified MOF glass membrane with a mixed gas.
[0019] Preferably, the mixed gas is selected from any one of a hydrogen-helium mixed gas, a helium-nitrogen mixed gas, a helium-methane mixed gas, a carbon dioxide-methane mixed gas, a carbon dioxide-nitrogen mixed gas, and a propylene-propane mixed gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an X-ray diffraction characterization result diagram of the product M1 in Example 1 of the specific implementation mode of the present invention;
[0021] Figure 2 This is a scanning electron microscope characterization cross-sectional result diagram of the product C1 obtained in Example 1 of the specific embodiment of the present invention;
[0022] Figure 3 This is a scanning electron microscope characterization surface result diagram of product M1 in Example 1 of the specific implementation mode of the present invention;
[0023] Figure 4 This is a scanning electron microscope characterization cross-sectional result diagram of product M1 in Example 1 of the specific implementation mode of the present invention;
[0024] Figure 5 The water contact angle diagrams of products M1, M4 and C1 in Example 1 of the specific implementation mode of the present invention;
[0025] Figure 6 This is a graph showing the carbon dioxide / methane gas separation performance of product M1 in Example 2 of a specific implementation manner of the present invention under a wet environment. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.
[0027] It should be noted that the endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.
[0028] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, the terms with conventionally understood meanings are defined herein for the purpose of illustrating or facilitating reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available reagents and instruments is carried out in accordance with the schemes and parameters given by the manufacturer.
[0029] In the prior art, MOF membranes often have the defects of being difficult to prepare and being unsuitable for gas separation. Based on this, a specific embodiment of the present invention provides a fluorinated modified MOF glass membrane that is suitable for gas separation and has a simple preparation method.
[0030] The fluorinated modified MOF glass film provided in the specific embodiment of the present invention contains organic ligands and fluorine ligands, wherein the molar ratio of the organic ligands to the fluorine ligands is (25-80): (20-75).
[0031] In the above embodiment, the fluorine-containing ligand can be replaced by a halogen-containing ligand with similar properties, such as a chlorine-containing ligand, 4-chloroimidazole, 5-chloro-1-methylimidazole, etc., or replaced by a bromine-containing ligand, 2-bromobenzimidazole, 4-bromo-1-H-imidazole, etc.
[0032] In the fluorinated modified MOF glass film provided in the above embodiment, the organic ligand is selected from any one or more of imidazole-2-carboxaldehyde, 2-methylimidazole, benzimidazole, 2-aminobenzimidazole, 4,5-dichloroimidazole, 2-nitroimidazole, 4-methylimidazole-5-carboxaldehyde.
[0033] In the fluorinated modified MOF glass film provided in a specific embodiment of the present invention, the metal frame is zinc element and / or cobalt element.
[0034] The specific embodiment of the present invention also provides a method for preparing the aforementioned fluorinated modified MOF, which specifically comprises the following steps:
[0035] S1: Preparation of MOF membrane;
[0036] S2: heating the fluorine-containing imidazole ligand to generate fluorine-containing vapor, which contacts the MOF membrane to form a MOF-F glass membrane;
[0037] S3: activating the MOF-F modified membrane in an activator to obtain a fluorinated modified MOF glass membrane.
[0038] In step S1 of the above embodiment, the method for preparing the MOF membrane may be a conventional method for preparing MOF.
[0039] Specifically, in step S1 of the above embodiment, the MOF membrane is preferably any one of ZIF-8, high-flux ZIF-8, ZIF-7, ZIF-93, ZIF-67, and ZIF-90, and more preferably any one of ZIF-8, high-flux ZIF-8, and ZIF-90.
[0040] ZIF-8 adopts the dip-coating thermal conversion method to prepare ZIF-8 membrane (patent CN 111841333 B). The ZIF-8 membrane prepared by this method has simple synthesis, high reproducibility, and excellent separation selectivity for macromolecular gases propylene and propane. By further reducing the concentration of the precursor solution, a high-throughput ZIF-8 membrane can be prepared (paper J.Membr.Sci.643(2022)
[0041] 120055). A high-throughput ZIF-8 membrane was prepared by controlling the concentration of the precursor solution, and the fluorine ligand vapor treatment conversion was carried out under the high-throughput ZIF-8 membrane, thereby improving the gas permeability.
[0042] Further, the preparation method of the ZIF-90 membrane specifically includes the following steps: dissolving 0.577g of imidazole-2-carboxaldehyde in 15ml of methanol at 80°C, adding 0.66g of zinc acetate dihydrate after cooling to room temperature, stirring in an ice bath for 8min to obtain a ZIF-90 precursor solution, dipping the carrier in the precursor solution for 30s, taking it out and drying the water, reacting it in a 50°C blast oven for 30min, and naturally cooling to obtain a ZIF-90 amorphous layer, and steaming the ZIF-90 amorphous layer in a DMF solution at 80°C for 12h to obtain a ZIF-90 membrane. The ZIF-90 membrane is prepared by a steam conversion method (Chem. Eng. J. 496 (2024) 153737), and the ZIF-90 membrane prepared by this method has excellent separation performance for n-isobutane and propylene propane. In step S2 of the above embodiment, the fluorine-containing ligand is selected from any one or more of monofluoromethylimidazole, difluoromethylimidazole, trifluoromethylimidazole, and 2-methyl-4-fluoroimidazole.
[0043] In step S2 of the above embodiment, the heating temperature for heating the fluorine-containing imidazole ligand to generate fluorine-containing steam is 60 to 100°C, and the contact time between the fluorine-containing steam and the MOF membrane is 6 to 48 hours. The heating temperature is preferably 60°C, 80°C, and 100°C. The optimal heating temperature is 80°C, and the heating methods include heating in a reactor, heating in air, and heating in a vacuum environment. Heating in a reactor is most preferred.
[0044] In step S3 of the above embodiment, the activator is selected from any one or more of dichloromethane, chloroform, dimethylformamide, methanol, ethanol, chloroform, acetone and acetonitrile. Unless otherwise specified, the activation described in the specific embodiment of the present invention is in accordance with conventional understanding, that is, the product to be activated is immersed in the activator for a period of time, and the activation time is 0.5 to 24 hours, preferably 1 to 12 hours, and most preferably 3 to 6 hours.
[0045] The fluorinated modified MOF glass membrane provided in the specific embodiment of the present invention is improved based on the MOF membrane in the prior art. Even after the MOF membrane comes into contact with fluorine-containing steam, fluorine element is doped into the MOF membrane, which reduces the pore size of the MOF membrane and greatly improves the gas selectivity of the MOF membrane. At the same time, the incorporation of fluorine element increases the water contact angle of the MOF membrane, which makes the fluorinated modified MOF glass membrane provided in the specific embodiment of the present invention still have good stability even in an environment with high humidity.
[0046] The technical solution of the present invention is further described below through specific embodiments.
[0047] Example 1
[0048] Preparation of fluorinated ZIF-8 glass membrane
[0049] 1.32 g (15 mmol) of Zn(OAc)2·2H2O and 1 g of 2-methylimidazole (30 mmol) were added to 15 ml of H2O / DMAC (2 / 1) solution, marked as solution A and solution B, respectively. After stirring in an ice bath for 8 minutes, solution B was added to solution A within 90 s. After stirring for 30 s, a precursor solution of ZIF-8 membrane was obtained. The Al2O3 carrier was dipped in the precursor solution for 30 s, taken out and dried, and reacted in a 200°C forced air oven for 15 min. After natural cooling, ZIF-8 polycrystalline membranes were obtained, which were marked as C1 to C6, respectively.
[0050] Take 0.2g of 4-trifluoromethylimidazole and place it in a small bottle. Invert the surface of the C1-C3 membrane (not in direct contact with the ligand), and react in a 70℃ forced air oven for 12h. C3-C6 react in an 80℃ forced air oven for 12h.
[0051] C1-C6 were taken out, activated in 10 ml of chloroform for 2 h, and vacuum activated in a vacuum oven at 100° C. for 12 h, and were respectively recorded as products M1-M6.
[0052] Characterization of fluorinated ZIF-8 glass membrane: XRD and SEM characterizations of the products M1 to M3 prepared above were performed, and the separation selectivity and permeability were measured. The XRD characterization results of product M4 are shown in the figure. Figure 1 As shown in Figure 2, after fluorination modification, the polycrystalline structure of ZIF-8 disappears and becomes an amorphous MOF glass structure. The SEM characterization results of product M1 are shown in Figure 2. Figure 3 As shown; the SEM characterization results of the product and M4 are shown in Figure 4 As shown in Figure 2, after fluorination modification, the regular polyhedral structure of the ZIF-8 surface disappears and transforms into an amorphous glass structure; the water contact angles of products M1 and M4 are shown in Figure 2. Figure 5 As shown in the figure, with the increase of fluorine content, the water contact angle increases, indicating that the incorporation of fluorine enhances the hydrophobicity of the membrane. According to the determination of H-NMR spectrum, the incorporation amount of fluorine ligand in product M1 is 22%, the ratio of 2-methylimidazole to 4-trifluoromethylimidazole of ZIF-8 ligand before modification is 78:22, and the incorporation amount in M4 is 58%.
[0053] The results of the separation selectivity and permeability of carbon dioxide / methane and carbon dioxide / nitrogen of products C1~C3 and M1~M3 are shown in Table 1-1, Table 1-2, Table 1-3. As shown in Table 1-4, when the doping amount is low, the fluorinated ZIF-8 glass membrane has excellent separation performance of carbon dioxide and methane and carbon dioxide / nitrogen. The volatilization temperature of the fluorinated imidazole ligand is further improved. When the doping amount is high, the separation selectivity and permeability of the fluorinated ZIF-8 glass membrane for hydrogen / methane and helium / nitrogen are shown in Table 1-5, Table 1-6, Table 1-7, Table 1-8. The fluorinated ZIF-8 glass membrane with a high doping amount has excellent separation performance of hydrogen and methane and helium and nitrogen.
[0054] Table 1-1: Results of carbon dioxide / methane separation selectivity and permeability test for C1 to C3
[0055]
[0056] Table 1-2: Carbon dioxide / methane separation selectivity and permeability test results of products M1~M3
[0057]
[0058] Table 2-3: Carbon dioxide / nitrogen separation selectivity and permeability test results of C1~C3
[0059]
[0060] Table 1-4: Carbon dioxide / nitrogen separation selectivity and permeability test results of products M1~M3
[0061]
[0062] Table 3-5: Hydrogen / methane separation selectivity and permeability test results of C4~C6
[0063]
[0064] Table 4-6: Hydrogen / methane separation selectivity and permeability test results of M4~M6
[0065]
[0066] Table 5-7: Helium / nitrogen separation selectivity and permeability test results of C4~C6
[0067]
[0068]
[0069] Table 6-8: Helium / nitrogen separation selectivity and permeability test results of M4~M6
[0070]
[0071] Example 2
[0072] Fluorinated ZIF-8 glass film tested in humidity environment
[0073] M1 to M3 in Example 1 were tested under a wet environment, a mixed gas of carbon dioxide and methane was introduced into water, and the mixed gas carrying water vapor was separated and tested on the membrane surfaces of M1 to M3.
[0074] The carbon dioxide-methane separation selectivity and permeability of products M1-M3 were measured under a humid environment. The separation selectivity and permeability test results of M1-M3 under a humid environment are shown in Table 2 and Attached Figure 6 As shown in Table 2, it can be seen that under humidity conditions, the permeability of the fluorinated ZIF-8 glass membrane is slightly reduced, but it still maintains a good separation selectivity.
[0075] Table 2: Results of CO2 / Methane separation selectivity and permeability test under humidity environment for M1~M3
[0076]
[0077] Example 3
[0078] High-throughput preparation of fluorinated ZIF-8 glass membrane
[0079] 0.33 g Zn(OAc)2·2H2O and 0.25 g 2-methylimidazole were added to 15 ml H2O / DMAC (2 / 1) solution, marked as solution A and solution B, respectively. After stirring in an ice bath for 8 minutes, solution B was added to solution A within 90 seconds. After stirring for 30 seconds, a precursor solution of a high-flux ZIF-8 membrane was obtained. The Al2O3 carrier was dipped in the precursor solution for 30 seconds, taken out and dried, and reacted in a forced air oven at 200°C for 15 minutes. After natural cooling, high-flux fluorinated ZIF-8 glass membranes were obtained, marked as C7, C8, and C9, respectively.
[0080] 0.2 g of 4-trifluoromethylimidazole was placed in a small bottle, and the surfaces of the C7, C8, and C9 membranes were inverted (not in direct contact with the ligands), and the reaction was carried out in a forced air oven at 80° C. for 12 h.
[0081] C7 to C9 were taken out, activated in 10 ml of chloroform for 2 h, and vacuum activated in a vacuum oven at 100° C. for 12 h. They were respectively recorded as product M7, product M8, and product M9.
[0082] The results of the carbon dioxide / methane separation selectivity and permeability test of products M7 to M9 are shown in Table 3. It can be seen that the high-flux ZIF-8 glass membrane after fluorination modification has excellent carbon dioxide / methane separation performance.
[0083] Table 3-1: Results of carbon dioxide / methane separation selectivity and permeability test for C7 to C9
[0084]
[0085] Table 3-2: Test results of carbon dioxide / methane separation selectivity and permeability of products M7~M9
[0086]
[0087] Example 4
[0088] Preparation of fluorinated ZIF-90 glass membrane
[0089] 0.577g of imidazole-2-carboxaldehyde was dissolved in 15ml of methanol at 80°C, cooled to room temperature, added with 0.66g of zinc acetate dihydrate, stirred in an ice bath for 8min to obtain a ZIF-90 precursor solution, and the Al2O3 carrier was dipped in the precursor solution for 30s, taken out and dried, and reacted in a 50°C forced air oven for 30min, and naturally cooled to obtain a ZIF-90 amorphous layer. The ZIF-90 amorphous layer was treated with steam at 80°C in DMF solution for 12h to obtain a ZIF-90 polycrystalline film, marked as C 10 , C11 and C 12 .
[0090] Take 0.2g of 4-trifluoromethylimidazole and place it in a small bottle. 10 , C 11 , C 12 The membrane surface was inverted (not in direct contact with the ligand) and reacted in a forced air oven at 80°C for 12 h.
[0091] C 10 ~C 12 Take it out, activate it in 10 ml of chloroform for 2 h, and activate it in a vacuum oven at 100 ° C for 12 h, which are respectively recorded as product M 10 , Product M 11 and product M 12 .
[0092] The test results of propylene / propane separation selectivity and permeability of products M4 to M6 are shown in Table 2. After fluorination modification, the propylene / propane separation performance of the fluorinated ZIF-90 glass membrane is significantly improved.
[0093] Table 4-1: C 10 ~C 12 Propylene / propane separation selectivity and permeability test results table
[0094]
[0095] Table 4-2: Product M 10 ~M 12 Propylene / propane separation selectivity and permeability test results table
[0096]
[0097] It can be seen from the experimental results of Examples 1 to 4 that the fluorinated MOF glass membrane provided by the specific embodiment of the present invention has a smaller pore size than the pure MOF membrane, thereby achieving the separation of specific gases.
[0098] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A fluorinated MOF glass film, characterized in that: The fluorinated modified MOF glass film contains organic ligands and fluorine ligands, wherein the molar ratio of the organic ligands to the fluorine ligands is (25-80): (20~75)。 2. The fluorinated MOF glass film according to claim 1, characterized in that: The organic ligand is selected from any one or more of imidazole-2-carboxaldehyde, 2-methylimidazole, benzimidazole, 2-aminobenzimidazole, 4,5-dichloroimidazole, 2-nitroimidazole, and 4-methylimidazole-5-carboxaldehyde.
3. A method for preparing the fluorinated MOF glass film according to claim 1 or 2, characterized in that: The following steps are involved: S1: Preparation of MOF membrane; S2: heating the fluorine-containing imidazole ligand to generate fluorine-containing vapor, which contacts the MOF membrane to form a MOF-F glass membrane; S3: activating the MOF-F glass film in an activator to obtain a fluorinated modified MOF glass film.
4. The preparation method according to claim 3, characterized in that: In the step S2, the fluorine-containing ligand is selected from any one or more of monofluoromethylimidazole, difluoromethylimidazole, trifluoromethylimidazole, and 2-methyl-4-fluoroimidazole.
5. The preparation method according to claim 3, characterized in that: In the step S2, the heating temperature for heating the fluorine-containing imidazole ligand to generate fluorine-containing steam is 60-100°C.
6. The preparation method according to claim 3, characterized in that: In the step S2, the contact time between the fluorine-containing steam and the MOF membrane is 6 to 48 hours.
7. The preparation method according to claim 3, characterized in that: In the step S3, the activating agent is selected from any one or more of dichloromethane, chloroform, dimethylformamide, methanol, ethanol, chloroform, acetone, acetonitrile, chloroform, acetone, and dimethylformamide.
8. The preparation method according to claim 3, characterized in that: In the step S3, the activation time is 0.5 to 24 hours.
9. An application of the fluorinated modified MOF glass film according to claim 1 or 2, characterized in that: Fluorinated MOF glass membranes were used for mixed gas separation.
10. The use according to claim 9, characterized in that The mixed gas is selected from any one of a hydrogen-helium mixed gas, a helium-nitrogen mixed gas, a helium-methane mixed gas, a carbon dioxide-methane mixed gas, a carbon dioxide-nitrogen mixed gas, and a propylene-propane mixed gas.
Citation Information
Patent Citations
Two fluorinated metal organic framework materials and preparation and low-carbon hydrocarbon separation application thereof
CN111072987A
Preparation method of sponge aluminum-based composite material for oil-gas separation
CN111871007A
Auto-polymerization microporous polymer fluorinated membrane as well as preparation method and application thereof
CN113337095A
Preparation method of fluorinated ZIF-90 modified PDMS film
CN114146582A
Organic skeleton gas separation membrane of zeolite iminazole metalloid
CN204768300U
Cited By
MOF-CGC material as well as preparation method and application thereof
CN119505275A
MOF glass as well as preparation method and application thereof
CN120423781A
A kind of MOF glass and its preparation method and application
CN120423781B