Preparation method and application of Ru monatomic noble metal type catalyst RuCeTi

By achieving single-atom-level dispersion of RuO2 and the interaction between CeO2 and TiO2 on CeTi support, the problem of insufficient thermal stability and anti-toxicity of catalysts is solved, the catalytic oxidation efficiency and thermal stability of chlorobenzene are improved, and high efficiency is achieved oxidation removal of chlorobenzene reduces the amount and cost of precious metals.

CN119016046AInactive Publication Date: 2024-11-26TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411228899.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing catalysts are prone to aggregation of precious metals at high temperatures, reducing catalytic effects, and the oxidation removal efficiency of volatile organic pollutants such as chlorobenzene is low, and the thermal stability and anti-toxicity are insufficient.

Method used

CeTi bimetallic oxide is used as a support to achieve single-atom dispersion of RuO2 through RuCl3 and NaBH4, and the interaction between CeO2 and TiO2 is used to increase the number of oxygen vacancies and electron environment of the catalyst, forming acidic sites to enhance catalytic activity.

Benefits of technology

Improve the thermal stability and anti-toxicity of the catalyst, enhance the catalytic oxidation activity of parachlorobenzene, and can efficiently convert chlorobenzene to CO2, H2O and HCl at lower temperatures, reduce the formation of dioxins, and reduce the Use of precious metals to reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016046A_ABST
    Figure CN119016046A_ABST
Patent Text Reader

Abstract

The invention relates to the field of chemical catalysts, and discloses a preparation method of a Ru monatomic noble metal catalyst RuCeTi, which comprises the following steps: mixing 2-5 ml of glacial acetic acid and 30-50 ml of absolute ethyl alcohol, adding 0.01-0.03 mol of tetrabutyl titanate, violently stirring for 10-20 minutes, and adding dilute nitric acid to adjust the pH value to 3-5 to obtain a solution A; 2-5 ml of deionized water and 15-25 ml of ethyl alcohol are mixed, 0.01-0.03 mol of cerium nitrate hexahydrate is added, stirring is conducted till solids are completely dissolved, and a solution B is obtained; slowly adding the solution B into the solution A, violently stirring for 30 minutes to 2 hours, then evaporating for 20 to 40 minutes at the temperature of 70 to 90 DEG C until the solution is in a sol state, drying in a blast oven, and then calcining in air in a tube furnace to obtain the CeTi carrier. According to the RuCeTi catalyst disclosed by the invention, RuCl3 is used as a precursor and NaBH4 is used as a reducing agent, so that the uniform dispersion of monatomic-level Ru noble metal on a CeTi bimetallic oxide carrier is realized, and the adsorption and catalytic oxidation efficiency of CVOCs (Chemical Volatile Organic Compounds) such as chlorobenzene and the like is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical catalysts, and in particular to a preparation method of a Ru single-atom noble metal catalyst RuCeTi and application thereof. Background Art

[0002] In many industrial activities, especially in the coking, steel and spraying industries, a large amount of volatile organic pollutants (VOCs) are emitted, which cause significant harm to the environment and human health. Chlorinated Volatile Organic Compounds (CVOCs), as a type of VOCs, are considered to be pollutants that need to be controlled first due to their high toxicity, difficulty in biodegradation and bioaccumulation. CVOCs can be produced in the process of incineration of garbage or waste, metallurgical industry, etc., and can be converted into dioxins that are more difficult to decompose at high temperatures of 200-400℃, thus causing serious diseases such as cancer or organ deformities.

[0003] In order to effectively control the emission of CVOCs, catalytic combustion technology is widely used in industrial emission control. This technology uses a catalyst to convert CVOCs into CO at a certain temperature. 2 , H 2 O, HCl and other low-toxic or non-toxic substances. Catalytic combustion equipment has the advantages of simple structure, convenient operation, stable performance and applicability to a wide range of CVOCs concentrations.

[0004] In the catalytic combustion process, the selection of catalysts is crucial. Precious metal-supported catalysts have become the preferred materials due to their high activity and low reaction temperature characteristics. Commonly used precious metals include gold (Au), palladium (Pd), platinum (Pt) and ruthenium (Ru). By reducing the size of precious metals to the atomic level, the active sites of the catalyst can be significantly increased without increasing the amount of precious metals, thereby improving the catalytic efficiency and saving costs. However, during the synthesis or catalytic reaction of the catalyst, the intensive heat exchange and the migration and diffusion of reactants and products may cause the precious metals to aggregate, thereby reducing the catalytic effect.

[0005] Based on the above background, the present invention provides a method for preparing a single-atom noble metal catalyst RuCeTi using a CeTi bimetallic oxide as a carrier to solve the deficiencies of the prior art. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing a Ru single-atom noble metal catalyst RuCeTi and its application, aiming to provide acidic sites and active sites that are beneficial to the chemical adsorption of CVOCs.3 As the precious metal source, NaBH4 as the reducing agent realizes the close combination of precious metal Ru and CeTi carrier, and forms a monodispersed RuO on the carrier surface. 2 Precious metals. CeO 2 With TiO 2 The interaction causes the ion valence state of Ru to change, increasing the number of oxygen vacancies in the catalyst, thereby enhancing the catalytic oxidation activity and tolerance of chlorobenzene. It has stronger thermal stability, anti-poisoning ability and ability to decompose chlorobenzene than the existing technology, providing a new and effective means for the oxidative removal of chlorobenzene.

[0007] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a Ru single-atom noble metal catalyst RuCeTi, comprising the following steps: Mix 2-5 ml of glacial acetic acid with 30-50 ml of anhydrous ethanol, add 0.01-0.03 mol of tetrabutyl titanate, stir vigorously for 10-20 minutes, add dilute nitric acid to adjust the pH to 3-5 to obtain solution A; mix 2-5 ml of deionized water with 15-25 ml of ethanol, add 0.01-0.03 mol of cerium nitrate hexahydrate, stir until the solid is completely dissolved to obtain solution B; slowly add solution B to solution A and stir vigorously for 30 minutes to 2 hours, then evaporate at 70-90°C for 20-40 minutes to a sol state, put into a blast oven to dry, and then calcine in air in a tube furnace to obtain a CeTi carrier; Prepare 0.5-2 mg / ml RuCl 3 The solution should be stored away from light; Dissolve 10-30 mg of sodium borohydride in 40-60 mL of deionized water for later use; Place 400-600 mg of CeTi support in a beaker, add 40-60 mL of deionized water, sonicate for 20-40 minutes, then add RuCl 3 4-6 mL of the solution was vigorously stirred for 30 minutes to 2 hours, sodium borohydride solution was added and continued to be stirred for 30 minutes to 2 hours, then filtered and washed with deionized water; the dried sample was dried at 90-110°C for 6-10 hours, and finally calcined in an air atmosphere at 300-400°C for 1-3 hours to obtain a RuCeTi catalyst.

[0008] Preferably, the drying temperature of the blast oven is 90-110° C. and the drying time is 6-10 hours.

[0009] Preferably, the calcination temperature in the tubular furnace is 300-400° C. and the calcination time is 1-3 hours.

[0010] Preferably, the catalyst RuCeTi prepared by the preparation method of Ru single atom noble metal type catalyst RuCeTi is characterized in that in the catalyst RuCeTi, the noble metal RuO 2 It is loaded on a CeTi carrier in an atomically dispersed state, wherein the CeTi carrier is prepared by a sol-gel method, and the precious metal Ru forms a strong interaction with the Ce element during the loading process.

[0011] Preferably, CeTi in the catalyst RuCeTi is a carrier, which provides acidic sites for adsorbing CVOCs and promotes the conversion of Ru to a high-valent state, while generating bimetallic oxides with oxygen vacancies.

[0012] Preferably, the mass fraction of Ru in the catalyst RuCeTi is 0.5% to 2% to ensure that the Ru element can exist in a single-atom form in the loaded material.

[0013] Preferably, the sodium borohydride solution is used to reduce RuCl 3 Ru in solution 3 + to Ru0, so as to facilitate its loading on the CeTi carrier in the form of single atom.

[0014] Preferably, the catalyst RuCeTi is used in the oxidation removal of chlorobenzene.

[0015] The present invention provides a preparation method and application of Ru single atom noble metal catalyst RuCeTi, which has the following beneficial effects: 1. The RuCeTi catalyst of the present invention is prepared by using RuCl 3 As a precursor and NaBH 4 As a reducing agent, the Ru noble metal at the single-atom level was evenly dispersed on the CeTi bimetallic oxide support. This atomic-level dispersion not only increases the active sites on the catalyst surface, but also provides more acidic sites that are conducive to the chemical adsorption of CVOCs, thereby improving the adsorption and catalytic oxidation efficiency of CVOCs such as chlorobenzene.

[0016] 2. CeO in the present invention 2 and TiO 2 The interaction between them forms a special electronic environment on the catalyst surface, causing the valence state of Ru to change. This valence change not only promotes the transfer of electrons, but also increases the number of oxygen vacancies in the catalyst, which are crucial for catalytic oxidation reactions because they can promote the oxidative decomposition of CVOCs such as chlorobenzene.

[0017] 3. Compared with the prior art, the RuCeTi catalyst of the present invention exhibits stronger thermal stability and can maintain structural integrity and catalytic activity even at high temperatures, which can reduce the aggregation and deactivation of precious metals and extend the service life of the catalyst. In addition, the catalyst's anti-poisoning ability has also been enhanced, and it can resist the influence of some common catalytic poisons, such as sulfur, chlorine and other elements, thereby maintaining efficient catalytic performance.

[0018] 4. The RuCeTi catalyst of the present invention exhibits higher catalytic oxidation activity for chlorobenzene and can achieve efficient conversion of chlorobenzene at a lower temperature, converting chlorobenzene into CO 2 , H 2 O and HCl, thereby reducing the risk of dioxin formation and having a more obvious protective effect on the environment and human health.

[0019] 5. Due to the high activity of the catalyst of the present invention, efficient catalytic performance can be achieved without increasing the amount of precious metals used, which means that the amount of precious metal catalysts used can be reduced in actual industrial applications, thereby reducing costs and improving economic benefits.

[0020] 6. The RuCeTi catalyst of the present invention is suitable for treating CVOCs in different concentration ranges due to its excellent thermal stability and anti-poisoning ability, which allows the catalyst to be used in a wider range of industrial scenarios and provides a more flexible and extensive environmental governance solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The HR-TEM images of the catalysts synthesized in Examples 6, 7 and 8 of the present invention are shown in Figure (a), wherein Figure (b) is RuCe, Figure (c) is RuTi, and Figure (d) is RuCeTi. Figure 2 These are high-angle annular spherical aberration electron microscope dark field images (CS-HADDF-STEM) of the catalysts synthesized in Examples 6, 7 and 8 of the present invention, wherein (a) is RuCe, (b) is RuTi, and (c) is RuCeTi; Figure 3 is the X-ray diffraction pattern (XRD) of the catalysts synthesized in Examples 3, 6, 7 and 8 of the present invention; Figure 4 is the Ru 3d orbital X-ray photoelectron spectrum (XPS) of the catalysts synthesized in Examples 6, 7 and 8 of the present invention; Figure 5 It is the mineralization rate curve of Examples 3, 6, 7 and 8 of the present invention in the catalytic oxidation of chlorobenzene, wherein the initial concentration of chlorobenzene is 1000 ppm and the space velocity is 15000 mL / (gh).

[0022] Figure 6 1 is the catalytic stability curve of Examples 3, 6, 7 and 8 of the present invention in the catalytic oxidation of chlorobenzene, wherein the initial concentration of chlorobenzene is 1000 ppm, the space velocity is 15000 mL / (gh), and the reaction time is 24 h. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1: Preparation of CeO 2 Carrier: First, Ce (NO 3 ) 3 6H 2 O (1.736 g, 4 mmol) and sodium hydroxide (19.2 g, 0.48 mol) were mixed and then dissolved in 80 mL of deionized water. After stirring for 30 min, the resulting solution was transferred to a 100 mL Teflon-lined stainless steel autoclave and reacted at 100 °C for 24 h, followed by centrifugation and washing. Finally, the obtained product was dried at 60 °C overnight and calcined at 400 °C in air for 2 h. The obtained powder was named CeO 2 .

[0025] Example 2: Preparation of TiO 2 Support: First, 0.02 mol (6.7383 g) of tetrabutyl titanate and 40 ml of anhydrous ethanol were mixed and stirred for 30 min to obtain solution A; 3 mL of glacial acetic acid, 20 mL of anhydrous ethanol, and 3 mL of deionized water were mixed, and dilute nitric acid (5 ml of concentrated nitric acid + 300 mL of water) was added to adjust the pH to 4, which was recorded as solution B; B was slowly added to solution A with a dropper to obtain a light yellow transparent gel and then stirred for 1 h, and then continued to stir in an 80 °C water bath environment until the light yellow gel turned into a transparent gel, and then placed in a 100 °C forced air oven to dry for 8 h, and then heated to 350 °C in a tubular furnace and calcined in air for 2 h. Finally, the obtained solid particles were recorded as TiO 2 ; Example 3: Preparation of CeTi bimetallic catalyst carrier: First, 3 ml of glacial acetic acid (AR, analytical grade) and 40 ml of anhydrous ethanol (AR, analytical grade) were mixed, and 0.02 mol (6.7383 g) of tetrabutyl titanate (≥99.0%) was added and stirred vigorously for 15 minutes, and dilute nitric acid (5 ml of concentrated nitric acid + 300 mL of water) was added to adjust the pH to 4, which was recorded as solution A; 3 ml of deionized water and 20 ml of ethanol were mixed, and 0.02 mol (8.6844 g) of cerium nitrate hexahydrate was added and stirred until the solid was completely dissolved, which was recorded as solution B; B was slowly added to solution A and stirred vigorously for 1 hour, and then evaporated at 80 ° C for 30 min until it was in a sol state and placed in a 100 ° C forced oven to dry for 8 hours, and then heated to 350 ° C in a tubular furnace and calcined in air for 2 hours, and finally the obtained solid particles were recorded as CeTi; Example 4: RuCl 3 Mixed to 1 mg / mL RuCl 3 Solution.

[0026] Example 5: 20 mg NaBH 4 Dissolve in 50 mL of water to prepare 0.4 mg / mL NaBH 4 Solution.

[0027] Example 6: CeO prepared in Example 1 2 The catalyst carrier synthesizes the unit noble metal catalyst RuCe: CeO prepared in Example 1 2 500 mg of the product was placed in a beaker, 50 mL of deionized water was added, and then ultrasonicated for 30 min, and then the RuCl prepared in Example 4 was added. 3 After 5 mL of the solution was vigorously stirred for 1 h, NaBH prepared in Example 5 was added. 4 The solution was stirred for 1 h and then filtered and washed with deionized water. The filtered and washed sample was dried in a drying oven at 100 °C for 8 h. Finally, it was calcined in a tubular furnace at 350 °C in an air atmosphere for 2 h. The obtained catalyst powder was recorded as RuCe (Ru mass fraction was 1%).

[0028] Example 7: TiO prepared in Example 2 2 The catalyst carrier is used to synthesize the unit noble metal catalyst RuTi: the TiO 2 500 mg of the powder was placed in a beaker, 50 mL of deionized water was added, and then ultrasonicated for 30 min, and then the RuCl prepared in Example 4 was added. 3 After 5 mL of the solution was vigorously stirred for 1 h, NaBH prepared in Example 5 was added. 4The solution was stirred for 1 hour and then filtered and washed with deionized water. The filtered and washed sample was dried in a drying oven at 100 °C for 8 hours. Finally, it was calcined in a tubular furnace at 350 °C in an air atmosphere for 2 hours. The obtained catalyst powder was recorded as RuTi (Ru mass fraction was 1%).

[0029] Example 8: Synthesis of a unit noble metal catalyst RuCeTi using the CeTi bimetallic catalyst carrier prepared in Example 3: 500 mg of CeTi powder in Example 3 was placed in a beaker, 50 mL of deionized water was added, and ultrasonicated for 30 min, and then the RuCl prepared in Example 4 was added. 3 After 5 mL of the solution was vigorously stirred for 1 h, NaBH prepared in Example 5 was added. 4 The solution was stirred for 1 h and then filtered and washed with deionized water. The filtered and washed sample was dried in a drying oven at 100 °C for 8 h. Finally, it was calcined in a tubular furnace at 350 °C in an air atmosphere for 2 h. The obtained catalyst powder was recorded as RuCeTi (Ru mass fraction was 1%).

[0030] Example 9: The activity and stability of the catalyst are achieved by connecting a fixed bed reactor to a gas chromatograph equipped with two FID detectors and a nickel converter. 100 mg of sample (40-60 mesh) is placed in a quartz tube with an inner diameter of 8 mm. The catalyst is stabilized with quartz sand and quartz wool before and after. The gas flows from the upper part of the quartz tube to the lower part, and the temperature of the catalyst bed is measured by a thermocouple inserted into the quartz tube from above. Chlorobenzene gas is obtained by volatilization of liquid chlorobenzene. The volatilization amount is adjusted by a set of cooling circulation equipment, and the concentration and space velocity of chlorobenzene are adjusted by the flow rate of air. The chlorobenzene concentration is measured by the FID detector, CO 2 Detected by FID combined with nickel converter.

[0031] Figure 1 is a high-magnification transmission electron microscope spectrum of the catalysts synthesized in Examples 6, 7 and 8. Figure 1 The macroscopic morphology and dispersion state of the catalyst carrier can be seen, but the existence of RuOx nanoparticles or metallic titanium Ru cannot be seen. Further observation is required through spherical aberration electron microscopy, such as Figure 2 shown.

[0032] Figure 2 This is a high-angle annular spherical aberration electron microscope dark field image of the catalysts synthesized in Examples 6, 7 and 8. It can be seen that the atomically dispersed precious metal Ru is evenly distributed on the catalyst surface, indicating that we have successfully synthesized a Ru-based single-atom dispersed catalyst.

[0033] Figure 3 The XRD patterns of the catalysts synthesized in Examples 3, 6, 7 and 8 are shown in Table 1.2 The morphology was successfully loaded on the surface of RuTi and RuCeTi catalysts. Due to the high loading amount, agglomerated RuO 2 Combined with the analysis results of spherical aberration electron microscopy, it is shown that on the surface of RuTi and RuCeTi catalysts, RuO 2 coexist in aggregated and monodispersed forms; in addition, only CeO 2 The diffraction peak of the face-centered cubic fluorite structure with the carrier space group Fm-3m (PDF#43-1002) is not visible. 2 Crystal phase, indicating that Ru is in CeO 2 The dispersion on the carrier is high and the particle size is small. XRD results show that in the bimetallic carrier CeTi, CeO 2 The component helps the dispersion of Ru ions.

[0034] Figure 4 is the XPS spectrum of the catalysts synthesized in Examples 3, 6, 7 and 8. Figure 4 It can be seen that in RuTi, the 3d 3 / 2 and 3D 5 / 2 The characteristic peak of the orbital is located at 284.9 cm -1 and 280.4 cm -1 , corresponding to Ru 4+ ; Ru in RuCeTi is 3 d3 / 2 and 3D 5 / 2 The characteristic peak of the orbital is located at 284.9 cm -1 and 281.1 cm -1 , corresponding to Ru 4+ And Ru 5+ ; In RuCeTi, the 3d 3 / 2 and 3D 5 / 2 The characteristic peak of the orbital is located at 284.9 cm -1 and 282.3 cm -1 , corresponding to Ru 4 + And Ru 6+ XPS shows that CeO 2 The addition of and helps the Ru element to transform from a low-valence state to a high-valence state, indicating that the interaction between Ru and Ce elements is strong, and electron transfer can occur, leading to the change of the valence state of the two elements; since metallic Ru was not observed, it shows that the dispersion of precious metals in the catalyst is relatively high.

[0035] Figure 5 The CO of the catalysts synthesized in Examples 3, 6, 7 and 8 during the catalytic oxidation of chlorobenzene 2Mineralization rate curve. As a typical CVOCs, the key to the catalytic oxidation of chlorobenzene is whether the catalyst has sufficient anti-poisoning and carbon deposition capabilities. Therefore, in the catalytic oxidation process of chlorobenzene, CO 2 The mineralization rate is the focus of our attention. As can be seen from the figure, the mineralization rates are arranged from high to low as RuCe, RuCeTi, RuTi, and CeTi. This shows that the addition of Ce element improves the RuO 2 While the dispersion is good (XRD), the electron transfer generated by its interaction with the Ru element (XPS) can effectively promote the oxidation of chlorobenzene by the catalyst.

[0036] Figure 6 Figure 2 is the stability curve of the catalysts synthesized in Examples 3, 6, 7 and 8 in chlorobenzene. It can be seen from the figure that although the mineralization rate of RuCe is higher than that of RuCeTi, the activity of RuCe gradually decreases during the long-term test, while the activity of RuCeTi remains basically unchanged within 24 h. The results show that RuCe and TiO 2 The combined effect of TiO 2 It provides the catalyst with a large amount of acidity that is beneficial to the chemical adsorption of chlorobenzene and its products. At the same time, the electron transfer generated by the strong interaction between Ru-Ce provides a continuous source of power for the catalytic oxidation process of chlorobenzene.

[0037] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a Ru single-atom noble metal catalyst RuCeTi, characterized in that: The following steps are involved: Mix 2-5 ml of glacial acetic acid with 30-50 ml of anhydrous ethanol, add 0.01-0.03 mol of tetrabutyl titanate, stir vigorously for 10-20 minutes, and add dilute nitric acid to adjust the pH to 3-5 to obtain solution A; Mix 2-5 ml of deionized water with 15-25 ml of ethanol, add 0.01-0.03 mol of cerium nitrate hexahydrate, and stir until the solid is completely dissolved to obtain solution B; Slowly add solution B into solution A and stir vigorously for 30 minutes to 2 hours, then evaporate at 70-90°C for 20-40 minutes until it becomes a sol, put it into a forced air oven for drying, and then calcine in air in a tube furnace to obtain a CeTi carrier; Prepare 0.5-2 mg / ml RuCl3 solution and store in dark place; Dissolve 10-30 mg of sodium borohydride in 40-60 mL of deionized water for later use; Place 400-600 mg of CeTi support in a beaker, add 40-60 mL of deionized water, ultrasonicate for 20-40 minutes, then add 4-6 mL of RuCl3 solution and stir vigorously for 30 minutes to 2 hours, then add sodium borohydride solution and continue stirring for 30 minutes to 2 hours, filter and wash with deionized water; The dried sample was dried at 90-110° C. for 6-10 hours, and finally calcined at 300-400° C. in an air atmosphere for 1-3 hours to obtain a RuCeTi catalyst.

2. The method for preparing a Ru single-atom noble metal catalyst RuCeTi according to claim 1, characterized in that: The drying temperature of the blast oven is 90-110° C. and the drying time is 6-10 hours.

3. The method for preparing a Ru single-atom noble metal catalyst RuCeTi according to claim 1, characterized in that: The calcination temperature in the tubular furnace is 300-400° C. and the calcination time is 1-3 hours.

4. The catalyst RuCeTi prepared by the preparation method of the Ru single atom noble metal type catalyst RuCeTi according to any one of claims 1 to 3, characterized in that: In the catalyst RuCeTi, the noble metal RuO2 is loaded on the CeTi carrier in an atomically dispersed state, wherein the CeTi carrier is prepared by a sol-gel method, and the noble metal Ru forms a strong interaction with the Ce element during the loading process.

5. A Ru single atom noble metal catalyst RuCeTi according to claim 4, characterized in that: In the catalyst RuCeTi, CeTi is a carrier, which provides acidic sites for adsorbing CVOCs, promotes the conversion of Ru to a high-valent state, and generates bimetallic oxides with oxygen vacancies.

6. The Ru single-atom noble metal catalyst RuCeTi according to claim 4, characterized in that: The mass fraction of Ru in the catalyst RuCeTi is 0.5% to 2% to ensure that the Ru element can exist in a single-atom form in the loaded material.

7. The method for preparing a Ru single-atom noble metal catalyst RuCeTi according to claim 1, characterized in that: The sodium borohydride solution is used to reduce Ru3+ in the RuCl3 solution to Ru0, so as to facilitate its loading on the CeTi carrier in the form of a single atom.

8. Use of the catalyst RuCeTi according to claims 1-7 in the oxidation removal of chlorobenzene.

Citation Information

Patent Citations

  • Preparation method of Ru / CeTiOX catalyst for low-temperature SCR (selective catalytic reduction) reaction

    CN106732581A

  • Monoatomic precious metal catalyst Ru / Cr2O3, preparation method and applications thereof

    CN110465291A

  • Cerium-based catalyst for efficiently degrading CVOCs

    CN115400745A

  • Preparation method and application of Ru monatomic noble metal type catalyst RuCeTi

    CN118179502A

  • Method for preparation of nanoceria supported atomic noble metal catalysts and the application of platinum single atom catalysts for direct methane conversion

    WO2019164797A1