Isomerization catalyst as well as preparation method and application thereof

Through ammonium fluorosilicate modified Y-type molecular sieve and active metal-supported catalyst, the problems of high toxicity, pollution and low catalyst activity in adamantane synthesis are solved, and high-efficiency and low-cost adamantane preparation is achieved, suitable for green and low-carbon chemicals. development.

CN119016092APending Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310579206.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing adamantane synthesis methods have problems such as high toxicity, serious pollution, low catalyst activity, and easy coking inactivation, resulting in low selectivity, high cost and serious pollution, which cannot meet the development trend of green and low-carbon chemicals.

Method used

The catalyst is prepared by ammonium fluorosilicate solution treatment and metal impregnation by using ammonium fluorosilicate modified Y-type molecular sieve and active metal-supported catalyst. Combined with hydrogen reduction, a bifunctional catalyst is formed for the isomerization of tetrahydrodicyclopentadiene. Prepare adamantane by chemical preparation.

Benefits of technology

It significantly improves the activity and stability of catalysts, reduces tar generation, improves the selectivity and conversion rate of adamantane, reduces production costs, is suitable for continuous production, and meets the requirements of green and low-carbon chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to an isomerization catalyst as well as a preparation method and application thereof. The isomerization catalyst is mainly composed of a Y-type molecular sieve and active metal, the preparation process comprises the following steps: firstly treating the Y-type molecular sieve with an ammonium fluosilicate solution, then loading metal and reducing to obtain the isomerization catalyst, and the isomerization catalyst can be used for a reaction of isomerizing tetrahydrodicyclopentadiene into adamantane. The Y molecular sieve is treated by ammonium fluosilicate, has the effects of molecular sieve pore expansion and acid amount and acid strength increase, and is further modified by the loaded metal, so that the catalyst has the characteristics of strong anti-coking capability, good stability and high activity when being used for catalyzing tetrahydrodicyclopentadiene to be isomerized into adamantane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an isomerization catalyst and a preparation method and application thereof. Background Art

[0002] Adamantane (ADH) is a highly symmetrical polycyclic cage hydrocarbon compound with the molecular formula C10H16. It has the characteristics of high density, good thermal stability and fat solubility. The hydrogen atoms on its ring can undergo substitution reactions and oxidation reactions, such as halogenation, nitration, sulfonation, etc. It has very wide applications in the synthesis of drug intermediates, molecular sieve catalysts, lubricating oils and the preparation of high-density liquid fuels.

[0003] At present, the raw material for synthesizing adamantane is tetrahydrodicyclopentadiene, as shown in the following formula. It can be directly obtained by isomerization of endo-tetrahydrodicyclopentadiene (endo-THDCPD), or further isomerized by exo-tetrahydrodicyclopentadiene (exo-THDCPD), a shallow isomerization product of endo-THDCPD.

[0004]

[0005] The main methods for synthesizing adamantane include aluminum chloride method, molecular sieve method, superacid method and ionic liquid method. The reaction mechanism is an acid-catalyzed carbon ion reaction, which requires acid as a catalyst. Olefin intermediates are also generated during the reaction. These olefin intermediates are prone to generate too many tar by-products under strong acid catalysis, which compete with the formation of adamantane, resulting in low selectivity for adamantane and serious material loss. However, when the acid strength used is not enough or the reaction conditions are too mild, the formation of adamantane cannot be promoted, and the selectivity of adamantane is also too low.

[0006] Among these methods, the aluminum chloride method has the characteristics of high conversion rate and high selectivity, with a conversion rate of more than 95% and a selectivity of 50%. The rest is mainly tar products. It is the current industrial method for producing adamantane. However, this method is a method for producing adamantane intermittently with a reactor as a reactor, and there are problems such as high toxicity, complex post-treatment, inability to recycle the catalyst, and large tar production in the process, resulting in low total output, high cost, and serious pollution in the production of adamantane by this method, which can no longer meet the development trend of green and low-carbon chemical industry in the future. The article "Synthesis of adamantane on commercially available zeolitic catalysts, Applied Catalysis A: General, 2000, 127-132" studied the preparation of adamantane by endo-THDCPD isomerization catalyzed by different molecular sieves. When Hβ was used as a catalyst, the yield of adamantane was 15.9%, but a large amount of tar was generated in the process, with a yield of 60%, which does not have the potential for industrial application. The article "Synthesis of adamantane on PW / USY composite catalyst, Journal of Advanced Chemical Engineering, 2007, 127-132." discloses that a PW / USY catalyst loaded with 10% phosphotungstic acid is used for isomerization of endo-THDCPD to adamantane, and a yield of 28.3% is obtained. However, the reaction is carried out in a reactor, and carbon is deposited on the surface of the PW / USY catalyst after each reaction, and high-temperature roasting and regeneration are required. The catalyst has poor anti-coking ability and does not have the ability of continuous production. Patent CN 1398245A discloses that a catalyst is made by loading a VIII group metal with a Y-type molecular sieve through an ion exchange method for the preparation of adamantane, and a continuous reaction is carried out in a stainless steel reaction tube. At 350°C, when the conversion rate of propylene norbornane (i.e., endo-THDCPD) is as high as 95.2%, the selectivity of adamantane is 12.8%, and there is room for further improvement in both the conversion rate and the selectivity. Summary of the invention

[0007] The present invention aims at the problems of high toxicity and high pollution in preparing adamantane by AlCl3 method and the problems of low catalyst activity and easy coking and deactivation in preparing adamantane by molecular sieve method, and provides a catalyst for preparing adamantane by isomerization of tetrahydrodicyclopentadiene.

[0008] The invention also provides a method for preparing adamantane.

[0009] A catalyst for preparing adamantane by isomerizing tetrahydrodicyclopentadiene mainly comprises a Y-type molecular sieve and an active metal. The catalyst preparation process comprises: firstly subjecting the Y-type molecular sieve to a modification treatment with an ammonium fluorosilicate solution, wherein the mass ratio of the ammonium fluorosilicate to the molecular sieve is 0.1 to 0.3, then impregnating the treated molecular sieve with a metal precursor, drying, calcining, and reducing in a reducing atmosphere to obtain the catalyst.

[0010] The Y-type molecular sieve is a hydrogen-type molecular sieve, preferably one or more of HY, HUSY, and REHY.

[0011] The mass fraction of Na2O contained in the Y-type molecular sieve is less than 0.5%, preferably less than 0.2%.

[0012] The Y-type molecular sieve is modified by an ammonium fluorosilicate solution. Preferably, the modification treatment conditions include: mixing the Y-type molecular sieve with water, stirring evenly to form a slurry, adding the ammonium fluorosilicate solution to the slurry of the Y-type molecular sieve according to the requirement that the mass ratio of ammonium fluorosilicate to the molecular sieve is 0.1 to 0.3, treating at 30 to 100° C., preferably 50 to 80° C., for 0.5 to 5 hours, preferably 0.5 to 3 hours, and then filtering and drying.

[0013] The metal is selected from one or more of Pt, Pd, Au, Ru, Rh, and Ni, and the metal precursor is a metal salt. When the metal is Pt, Pd, Au, Ru, or Rh, the metal loading is 0.05 to 5.0%, preferably 0.2 to 0.5%, and when the metal is Ni, the metal loading is 1.0 to 10%, preferably 3 to 6%.

[0014] The concentration of the ammonium fluorosilicate solution is 0.02-2 mol / L, preferably 0.05-0.3 mol / L.

[0015] The mass ratio of the Y-type molecular sieve to water is 1:1 to 1:30, preferably 1:5 to 1:15, so as to form a slurry.

[0016] The supported catalyst is further calcined at 350-600°C, preferably 400-500°C for 1-6h, preferably 2-4h; and reduced at 150-600°C, preferably 250-500°C, in a hydrogen atmosphere for more than 1h to obtain the isomerization catalyst.

[0017] A method for preparing adamantane, comprising: mixing tetrahydrodicyclopentadiene and a solvent in a reactor, and reacting in the presence of hydrogen and the above-mentioned isomerization catalyst, wherein the reaction temperature is 181-300°C, preferably 200-260°C; the reaction hydrogen pressure (gauge pressure) is 0.1-3.0 MPa, preferably 0.5-1.0 MPa; the mass space velocity is 0.2-5 h~1 , preferably 0.5 to 2 hours ~1 ; The hydrogen-to-hydrocarbon volume ratio is 100 to 3000, preferably 600 to 1200.

[0018] Preferably, the tetrahydrodicyclopentadiene is mixed with a solvent before the reaction, wherein the mass concentration of tetrahydrodicyclopentadiene in the mixed solution is 10 to 80 wt%, preferably 30 to 60 wt%; the solvent is a hydrocarbon or halogenated hydrocarbon solvent with a boiling point of 40 to 300° C., preferably C6 to C10 hydrocarbons, more preferably cyclohexane, methylcyclohexane, exo-tetrahydrodicyclopentadiene or a combination thereof.

[0019] The reactor can be a fixed bed reactor, a moving bed reactor, a fluidized bed, or a slurry bed, preferably a fixed bed reactor.

[0020] The method of the present invention prepares a metal / molecular sieve supported bifunctional catalyst. The molecular sieve is first treated with an ammonium fluorosilicate solution to achieve the effects of catalyst pore expansion and increased acid quantity and acid strength, thereby improving catalyst activity and stability. The catalyst is further impregnated with a metal to prepare a bifunctional catalyst. The catalyst has the characteristic of significantly inhibiting catalyst coking and deactivation, and can be used for isomerization of tetrahydrodicyclopentadiene to prepare adamantane. DETAILED DESCRIPTION

[0021] The specific implementation modes of the present invention are further described below in conjunction with examples.

[0022] In the embodiment:

[0023] Ammonium Fluorosilicate Source: Beijing Inokai Technology Co., Ltd.

[0024] Bridged Tetrahydrodicyclopentadiene Source: Beijing Inokai Technology Co., Ltd.

[0025] Examples 1-2 (Effect of Na2O Content in Molecular Sieve)

[0026] The HY molecular sieve with different Na2O contents was dried and then impregnated with metal Pt. The metal precursor was tetraamine platinum chloride with a loading of 0.3%. The isovolumetric impregnation method was used and the impregnation was carried out for 6 hours at room temperature. During the process, the catalyst was dried at 80°C, calcined at 450°C for 3 hours, and reduced with hydrogen at 400°C for 3 hours. The bifunctional catalyst with different Na2O contents was obtained and its catalytic activity was evaluated (results after 10 hours of reaction). Here, a methylcyclohexane solution containing 50wt% of bridged tetrahydrodicyclopentadiene (endo-THDCPD) was used as the raw material in a fixed bed reactor. The reaction temperature was 220°C, the reaction pressure (gauge pressure) was 0.5MPa H2, and the mass space velocity of endo-THDCPD was 1h ~1, the volume ratio of hydrogen to hydrocarbon is 1000, and the performance of the catalyst is investigated.

[0027]

[0028] Examples 3 to 5 (Effect of the amount of ammonium fluorosilicate used in treatment)

[0029] HY molecular sieve (Na2O content of 0.07%) was dried, and then the HY molecular sieve was mixed and stirred with water to form a slurry, and then treated with ammonium fluorosilicate. According to the requirements that the mass ratio of ammonium fluorosilicate to HY molecular sieve is 0, 0.1, 0.2, 0.3, and 0.4, 0.1 mol / L ammonium fluorosilicate solution was slowly added to the HY molecular sieve slurry, and then stood at 60°C for 1 hour, and finally washed and dried to obtain HY molecular sieves modified with different amounts of ammonium fluorosilicate, and the specific surface area, pore volume, mesoporous volume, acid content, etc. of the catalyst were further characterized and analyzed, and the metal loading and catalyst activity evaluation were performed according to the method described in Example 1 (results after 10 hours of reaction).

[0030]

[0031] Examples 6 to 12 (Effects of ammonium fluorosilicate concentration, treatment temperature and time)

[0032] The HY molecular sieve (Na2O content is 0.07%) is dried, and then the HY molecular sieve is mixed and stirred with water to form a slurry, and then treated with ammonium fluorosilicate according to the steps and proportions of Example 3, but the concentration of the ammonium fluorosilicate solution is adjusted to 0.05 mol / L or 0.3 mol / L. In addition, the treatment temperature of the ammonium fluorosilicate is adjusted to 50°C or 80°C, and the treatment time is adjusted to 0.5h or 3h. Then, the metal loading and catalyst activity evaluation are carried out according to the method described in Example 1 (the results after 10h of reaction).

[0033]

[0034]

[0035] Examples 13 to 16 (Effect of Metal Loading)

[0036] HY molecular sieve (Na2O content of 0.07%) was dried and then treated with ammonium fluorosilicate. According to the steps of Example 3, the ammonium fluorosilicate solution was slowly added to the HY molecular sieve slurry according to the requirement that the mass ratio of ammonium fluorosilicate to HY molecular sieve was 0.1, and then it was allowed to stand at 60°C for 1 hour, and finally washed and dried to obtain the HY molecular sieve modified with ammonium fluorosilicate, and then the metal loading and catalyst activity evaluation (results after 50 hours of reaction) were carried out according to the method described in Example 1, but the type and loading amount of the loaded metal were adjusted.

[0037]

[0038] Examples 17 to 20 (Effect of Reaction Temperature)

[0039] HY molecular sieve (Na2O content of 0.07%) was dried and then treated with ammonium fluorosilicate. According to the steps of Example 3, the ammonium fluorosilicate solution was slowly added dropwise to the HY molecular sieve slurry according to the requirement that the mass ratio of ammonium fluorosilicate to HY molecular sieve was 0.1, and then it was allowed to stand at 60°C for 1h, and finally washed and dried to obtain the HY molecular sieve modified with ammonium fluorosilicate, and then the metal loading and catalyst activity evaluation (results after 50h of reaction) were carried out according to the method described in Example 1, but the reaction temperatures were adjusted to 180°C, 260°C, and 300°C, respectively.

[0040]

[0041] Examples 21 to 23 (Effect of Reaction Hydrogen Pressure)

[0042] HY molecular sieve (Na2O content of 0.07%) was dried and then treated with ammonium fluorosilicate. According to the steps of Example 3, the ammonium fluorosilicate solution was slowly added dropwise to the HY molecular sieve slurry according to the requirement that the mass ratio of ammonium fluorosilicate to HY molecular sieve was 0.1, and then it was allowed to stand at 60°C for 1h, and finally the HY molecular sieve modified with ammonium fluorosilicate was obtained by washing and drying, and then the metal loading and catalyst activity evaluation (results after 10h of reaction) were carried out according to the method described in Example 1, but the reaction hydrogen pressure (gauge pressure) was adjusted to 0MPa, 0.5MPa, 1.0MPa, 2.0MPa.

[0043]

[0044] Examples 24 to 27 (Influence of reaction space velocity)

[0045] The HY molecular sieve (Na2O content of 0.07%) was dried and then treated with ammonium fluorosilicate. According to the steps of Example 3, the ammonium fluorosilicate solution was slowly added to the HY molecular sieve slurry according to the requirement that the mass ratio of ammonium fluorosilicate to HY molecular sieve was 0.1, and then it was allowed to stand at 60°C for 1 hour, and finally washed and dried to obtain the HY molecular sieve modified with ammonium fluorosilicate, and then the metal loading and catalyst activity evaluation (results after 10 hours of reaction) were carried out according to the method described in Example 1, but the mass space velocity of endo-THDCPD was adjusted to 0.5h ~1 , 1.0h ~1 , 2.0h ~1 , 4.0h ~1 .

[0046]

[0047] Examples 28 to 30 (Influence of reaction solvent)

[0048] HY molecular sieve (Na2O content of 0.07%) was dried and then treated with ammonium fluorosilicate. According to the steps of Example 3, the ammonium fluorosilicate solution was slowly added dropwise to the HY molecular sieve slurry according to the requirement that the mass ratio of ammonium fluorosilicate to HY molecular sieve was 0.1, and then it was allowed to stand at 60°C for 1h, and finally the HY molecular sieve modified with ammonium fluorosilicate was obtained by washing and drying, and then the metal loading and catalyst activity evaluation (result after 10h of reaction) were carried out according to the method described in Example 1, but the reaction solvent was replaced with hanging tetrahydrodicyclopentadiene, dichloromethane, and isopropanol.

[0049]

Claims

1. A catalyst for preparing adamantane by isomerization of tetrahydrodicyclopentadiene, comprising a Y-type molecular sieve and an active metal, wherein the catalyst preparation process comprises: The Y-type molecular sieve is first modified by an ammonium fluorosilicate solution, wherein the mass ratio of ammonium fluorosilicate to the molecular sieve is 0.1-0.3, and then the treated molecular sieve is impregnated with a metal precursor, dried, calcined, and reduced in a reducing atmosphere.

2. The catalyst according to claim 1, wherein The Y-type molecular sieve is a hydrogen-type molecular sieve, preferably one or more of HY, HUSY, and REHY.

3. The catalyst according to claim 1, wherein The mass fraction of Na2O contained in the Y-type molecular sieve is less than 0.5%, preferably less than 0.2%.

4. The catalyst according to claim 1, wherein The Y-type molecular sieve is modified by an ammonium fluorosilicate solution, wherein the modification conditions include: mixing the Y-type molecular sieve with water, stirring evenly to form a slurry, and adding the ammonium fluorosilicate solution to the slurry of the Y-type molecular sieve according to the requirement that the mass ratio of ammonium fluorosilicate to the molecular sieve is 0.1 to 0.

3.

5. The catalyst according to claim 1, wherein The modification treatment conditions include: treatment temperature of 30 to 100° C., preferably 50 to 80° C., treatment time of 0.5 to 5 hours, preferably 0.5 to 3 hours, filtering and drying after treatment.

6. The catalyst according to claim 1, wherein The metal is selected from one or more of Pt, Pd, Au, Ru, Rh, and Ni, and the metal precursor is a metal salt.

7. The catalyst according to claim 1, wherein When the metal is Pt, Pd, Au, Ru, or Rh, the metal loading is 0.05 to 5.0%, preferably 0.2 to 0.5%. When the metal is Ni, the metal loading is 1.0 to 10%, preferably 3 to 6%.

8. The catalyst according to claim 1, wherein The concentration of the ammonium fluorosilicate solution is 0.02-2 mol / L, preferably 0.05-0.3 mol / L.

9. The catalyst according to claim 1 and claim 4, wherein The mass ratio of the Y-type molecular sieve to water is 1:1 to 1:30, preferably 1:5 to 1:

15.

10. A method for preparing adamantane, comprising: Tetrahydrodicyclopentadiene is mixed with a solvent in a reactor, and reacted in the presence of hydrogen and a catalyst according to any one of claims 1 to 9, the reaction temperature is 181 to 300° C., preferably 200 to 260° C.; the reaction hydrogen pressure (gauge pressure) is 0.1 to 3.0 MPa, preferably 0.5 to 1.0 MPa.

11. The method according to claim 10, wherein: Mass space velocity is 0.2~5h ~1 , preferably 0.5 to 2 hours ~1 ; The volume ratio of hydrogen to hydrocarbon is 100 to 3000, preferably 600 to 1200.

12. The method according to claim 10, wherein: Before the reaction, the tetrahydrodicyclopentadiene is mixed with a solvent, and the mass concentration of the tetrahydrodicyclopentadiene in the mixed solution is 10 to 80 wt %, preferably 30 to 60 wt %.

13. The method according to claim 10, wherein: The solvent is a hydrocarbon or halogenated hydrocarbon solvent with a boiling point of 40 to 300° C., preferably a C6 to C10 hydrocarbon, more preferably cyclohexane, methylcyclohexane, exo-tetrahydrodicyclopentadiene or a combination thereof.

14. The method according to claim 10, wherein: The reactor can be a fixed bed reactor, a moving bed reactor, a fluidized bed, or a slurry bed, preferably a fixed bed reactor.

Citation Information

Patent Citations

  • Process for producing adamantane compound

    CN1398245A