Aluminum-lithium alloy material as well as preparation method and application thereof

By forming a dense aluminum film and an oxide film on the surface of aluminum-lithium alloy particles, the problem of easy oxidation of aluminum-lithium alloy is solved, its stability and safety are improved, efficient antioxidant effect is achieved, and production costs are reduced.

CN119016724APending Publication Date: 2024-11-26XIANGTAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411085868.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The easy oxidation of aluminum lithium alloys leads to poor stability and safety problems. The existing antioxidant technology is costly and is not conducive to large-scale application. It is difficult for traditional coating methods to form a uniform and dense protective layer.

Method used

A dense aluminum film is formed on the surface of aluminum lithium alloy particles, and the aluminum film is coated by magnetron sputtering process and an oxide film is formed on its outer layer to form an atomic diffusion layer to prevent oxygen contact and improve the stability of the material.

Benefits of technology

Effectively prevent oxidation reactions, significantly improve the corrosion resistance and thermal stability of aluminum-lithium alloys, extend service life, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016724A_ABST
    Figure CN119016724A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum-lithium alloy material which comprises aluminum-lithium alloy particles and an aluminum film coating the surfaces of the aluminum-lithium alloy particles, an oxidation film is formed on the surface of the aluminum film, a bonding interface is formed between the aluminum film and the aluminum-lithium alloy particles, an atomic diffusion layer is formed at the bonding interface, and the average particle size of crystal grains in the aluminum film is 42-126 nm. The invention further discloses a preparation method and application of the aluminum-lithium alloy material. According to the method, a layer of compact aluminum film is formed on the surface of the aluminum alloy, so that contact between oxygen and the aluminum-lithium alloy is effectively prevented, an oxidation reaction is prevented, and the stability of the aluminum-lithium alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum-lithium alloy and processing thereof, and in particular to an aluminum-lithium alloy material and a preparation method and application thereof. Background Art

[0002] Aluminum-lithium alloy metal fuel is an advanced metal fuel that combines the advantages of aluminum and lithium. It has the characteristics of low density, high specific strength and specific stiffness, excellent low-temperature performance and corrosion resistance. By utilizing the characteristics of aluminum-lithium alloy reacting with water, efficient and environmentally friendly hydrogen fuel can be prepared. This hydrogen fuel has wide application potential in fuel cells, hydrogen-powered vehicles and other fields. With the continuous advancement of science and technology and the continuous expansion of application fields, aluminum-lithium alloy metal fuel will show its unique advantages and application value in more fields.

[0003] Since lithium metal itself is a very active metal, it is very easy to react with oxygen in the air, resulting in oxidation; when lithium is added to aluminum alloy, this activity still exists and may even aggravate the oxidation process of aluminum alloy, which will not only affect the long-term storage stability of the fuel, but also may cause safety problems during use. In order to overcome the oxidizability of aluminum-lithium alloys, effective anti-oxidation technology needs to be developed. At present, methods such as sol coating and chemical coating have been proposed to improve the thermal stability of aluminum-lithium alloys. There are also methods such as electroplating and chemical vapor deposition to coat a protective layer on the surface of the alloy. These methods have improved the stability of aluminum-lithium alloys to a certain extent, but there are still some problems. First, traditional coating methods often cannot form a uniform and dense protective layer, resulting in film detachment and separation of aluminum-lithium alloys during pharmaceutical preparation or storage, and oxidation will still occur. Secondly, changing the composition of aluminum alloy or lithium alloy may affect its other properties, such as thermodynamic properties, ignition and combustion performance, etc. Then, the chemical vapor deposition coating atmosphere is toxic, which is not conducive to processing and production. In addition, existing solutions often require complex equipment and processes, with high costs, which are not conducive to large-scale applications. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the purpose of the present application is to provide an aluminum-lithium alloy material, which effectively prevents oxygen from contacting the aluminum-lithium alloy by forming a dense aluminum film on the surface of the aluminum alloy, thereby preventing the occurrence of oxidation reaction and improving the stability of the aluminum-lithium alloy.

[0005] To solve the above problems, the technical solutions adopted in this application are as follows: The present application provides an aluminum-lithium alloy material, comprising aluminum-lithium alloy particles and an aluminum film coated on the surface of the aluminum-lithium alloy particles, wherein an oxide film is formed on the surface of the aluminum film, a bonding interface is formed between the aluminum film and the aluminum-lithium alloy particles, an atomic diffusion layer is formed at the bonding interface, and an average particle size of grains in the aluminum film is 42~126nm.

[0006] As a further preferred solution, the atomic diffusion layer described in the embodiment of the present application is an aluminum-lithium element diffusion layer, and the proportion of aluminum element in the atomic diffusion layer is 91.2wt%~98.7wt%.

[0007] As a further preferred solution, the thickness of the atomic diffusion layer described in the embodiment of the present application is 120~200nm.

[0008] As a further preferred solution, the thickness of the aluminum film described in the embodiment of the present application is 0.3~0.8μm, and the thickness of the oxide film is 0.05~0.15μm.

[0009] The present application also provides a method for preparing an aluminum-lithium alloy material, which uses a magnetron sputtering process to form an aluminum film on the surface of an aluminum-lithium alloy particle. The specific steps are as follows: Pretreatment of aluminum-lithium alloy particles: Screening out impurities from vacuum-stored aluminum-lithium alloy particles in a protective atmosphere; Sputtering film formation: The screened aluminum-lithium alloy particles are placed in a magnetron sputtering device equipped with an aluminum target, and the sputtering parameters are set to coat the aluminum-lithium alloy particles, thereby wrapping a layer of aluminum film on the surface of the aluminum-lithium alloy; Aluminum film passivation treatment: The aluminum-lithium alloy particles wrapped with aluminum film are placed in a constant temperature and humidity phase for passivation treatment to form an oxide film on the outer layer of the aluminum film.

[0010] As a further preferred embodiment, in the preparation method described in the embodiment of the present application, the size of the aluminum-lithium alloy particles is 20-50 μm.

[0011] As a further preferred solution, in the preparation method described in the embodiment of the present application, the magnetron sputtering device is a rolling cylindrical structure, and a plurality of protrusions are arranged on the inner wall of the rolling cylindrical structure, and the plurality of protrusions are arranged equidistantly along the axial direction of the drum. Further, the protrusions are continuous gear-shaped protrusions or spaced tooth-shaped protrusions.

[0012] As a further preferred scheme, in the preparation method described in the embodiment of the present application, during sputtering film formation, the magnetron sputtering equipment is filled with protective gas, the sputtering power is set to 1.5~3.5Kw, the pressure is set to 0.3~0.8Mpa, and the sputtering time is 2~8h; the rotation speed of the rolling cylindrical structure is 2r / min.

[0013] As a further preferred scheme, in the preparation method described in the embodiment of the present application, during the passivation treatment of the aluminum film, the temperature is 55~65°C, the humidity is 72~85%, and the placement time is 20~30h.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The oxide film on the surface of the aluminum film of the aluminum-lithium alloy material described in this application is mainly composed of aluminum oxide, which has a dense and uniform structure and can effectively prevent external oxygen atoms from further reacting with the internal aluminum-lithium alloy, significantly improving the corrosion resistance of the material; the aluminum oxide layer effectively slows down the oxidation rate of the aluminum-lithium alloy in high temperature or oxidizing atmosphere, and prolongs the service life of the material.

[0015] 2. The average grain size of the aluminum film of the aluminum-lithium alloy material described in this application is controlled within the range of 40-120 nm, which can improve the compactness of the aluminum film. The fine grains help to disperse and hinder the movement of dislocations, resulting in higher strength, hardness and better plastic deformation ability.

[0016] 3. Furthermore, in the aluminum-lithium alloy material described in the present application, the atomic diffusion layer formed at the bonding interface between the aluminum film and the aluminum-lithium alloy particles enhances the bonding strength between the aluminum film and the aluminum-lithium alloy particles.

[0017] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0019] Figure 1 This is a schematic diagram of the aluminum-lithium alloy particle structure described in Example 1 of the present application; Figure 2 This is the SEM image of the original aluminum-lithium alloy particles; Figure 3 This is a SEM image of the aluminum-lithium alloy particles described in Example 1 of the present application.

[0020] Figure 4 This is a diagram of the bonding interface organization structure of the aluminum-lithium alloy material described in the embodiment of the present application. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0022] The term "comprising" and other equivalent descriptions involved in the specification and claims of this application are intended to cover non-exclusive inclusions, including both the contents clearly described in the specification and claims, and the steps or units that are not described in the specification and claims but are inherent in the product, method or structure.

[0023] The present application provides an aluminum-lithium alloy material, including aluminum-lithium alloy particles and an aluminum film coated on the surface of the aluminum-lithium alloy particles, wherein an oxide film is formed on the surface of the aluminum film, and a bonding interface is formed between the aluminum film and the aluminum-lithium alloy particles. At the contact interface between the aluminum film and the aluminum-lithium alloy particles, due to the presence of a concentration gradient or a temperature gradient, an atomic diffusion layer is formed at the aluminum-lithium bonding interface, which is mainly manifested as the aluminum element diffusing from a high concentration area to a low concentration area. Of course, during the diffusion process, the lithium element will also diffuse from the aluminum-lithium alloy particles into the aluminum film to form a lithium-rich area. After the aluminum film is coated, the atomic diffusion layer formed can serve as a barrier. On the one hand, it can hinder the rapid diffusion of atoms inside the aluminum-lithium alloy at high temperatures, which helps to maintain the structural stability of the material at high temperatures; on the other hand, it can prevent the aluminum-lithium alloy from reacting with oxygen at high temperatures to generate harmful products such as oxides to a certain extent; in addition, the good interface bonding force formed between the aluminum film and the aluminum-lithium alloy matrix helps to maintain the overall integrity of the material at high temperatures, and the enhancement of the interface bonding force can reduce the internal stress concentration and crack propagation of the material caused by temperature changes, thereby improving the thermal stability of the material. By controlling the proportion of aluminum, the structure and performance of the diffusion layer can be optimized, thereby improving the overall performance of the aluminum film coated aluminum-lithium alloy material. In some embodiments of the present application, the proportion of aluminum in the atomic diffusion layer is 91.2wt%~98.7wt%. The average grain size of the grains in the aluminum film has a positive effect on the bonding force between the aluminum film and the aluminum-lithium alloy and the coating effect. The smaller average grain size of the grains means that there are more grain boundaries and defects on the surface of the aluminum film. These areas may become active sites for the diffusion and reaction of aluminum atoms and aluminum-lithium alloy matrix atoms, that is, smaller grain size helps to increase the interface contact area and improve the bonding force between the aluminum film and the aluminum-lithium alloy; fine grains help to reduce stress concentration at the interface. When the aluminum film is combined with the aluminum-lithium alloy, due to the difference in the thermal expansion coefficient and elastic modulus between the two, stress is easily generated at the interface. The smaller grain size helps to disperse these stresses and reduce the risk of interface cracking; in addition, fine grains mean that the aluminum film has a higher density and is easy to form a more uniform coating layer. Therefore, in order to further increase the interface contact area, shorten the diffusion path, disperse the stress concentration, and improve the density and uniformity of the coating layer, the average grain size of the aluminum film is 42-126 nm.

[0024] In the research of this application, it is found that the thickness of the atomic diffusion layer has a significant effect on the bonding force between the aluminum film and the aluminum-lithium alloy and the coating effect. A thicker diffusion layer means that more atoms diffuse and combine at the interface, thereby forming a stronger metallurgical bond, which can significantly improve the bonding force between the aluminum film and the aluminum-lithium alloy, making it difficult for the two to separate when subjected to force. At the same time, a thicker diffusion layer is often accompanied by a denser coating layer, because the interaction between atoms during the diffusion process helps to fill the defects and pores in the coating layer; the dense coating layer can provide better protection and prevent the aluminum-lithium alloy matrix from being corroded by the external environment. However, the thickness of the atomic diffusion layer is not the thicker the better. An overly thick diffusion layer may cause too many intermetallic compounds or other brittle phases to form at the interface. These brittleness will reduce the bonding strength of the interface and weaken the bonding force between the aluminum film and the aluminum-lithium alloy. During the coating process, if the diffusion layer is too thick, the coating layer may become uneven or have defects (such as pores, cracks, etc.), thereby reducing the protective effect of the coating layer. Therefore, in order to ensure the bonding force between the aluminum film and the aluminum-lithium alloy particles and the coating effect, as a further preferred solution, in some embodiments of the present application, the thickness of the atomic diffusion layer is 120-200 nm. Preferably, the thickness of the atomic diffusion layer is 150-180 nm.

[0025] In the research of this application, it was found that the thickness of the aluminum film affects the thermal stability of the aluminum-lithium alloy particles. A thicker aluminum film can provide a better thermal barrier effect, reduce the direct thermal shock of the external environment to the aluminum-lithium alloy particles, and thus improve its thermal stability to a certain extent; but an overly thick aluminum film may also cause thermal stress concentration and increase the risk of cracking of the material during temperature changes. In addition, the thickness of the aluminum film will directly affect the thickness and composition of the oxide film on the surface of the aluminum-lithium alloy particles. The thicker aluminum film may slow down the direct contact between the aluminum-lithium alloy particles and oxygen to a certain extent, thereby increasing the ignition temperature; the thinner aluminum film may be more easily penetrated by heat, so that the aluminum-lithium alloy particles reach the reaction temperature faster during the combustion process, thereby increasing the combustion rate, but the overly thin aluminum film may also cause the aluminum-lithium alloy particles to be exposed to the high temperature environment prematurely during the combustion process, causing local overheating and ablation. Therefore, in order to optimize the performance of the aluminum-lithium alloy particles, as a further preferred solution, in some embodiments of the present application, the thickness of the aluminum film is 0.3~0.8μm.

[0026] In the present application, an oxide film and an aluminum oxide film are formed on the surface of the aluminum film. The aluminum oxide film can effectively isolate the direct contact between the air and the aluminum substrate, thereby slowing down or preventing further oxidation of the aluminum; the aluminum oxide film has the advantages of uniformity, density, high hardness, etc., and has stronger corrosion resistance and wear resistance. Thicker oxide films usually provide better heat insulation and enhance the thermal stability of alloy particles; however, an overly thick oxide film may produce greater thermal stress during temperature changes, increasing the risk of cracking of alloy particles. Therefore, in the present application, the thickness of the oxide film is 0.05~0.15μm. Preferably, the thickness of the oxide film is 0.1~0.12μm.

[0027] The aluminum-lithium alloy material described in the embodiment of the present application is to form an aluminum film on the surface of the aluminum-lithium alloy particles by a magnetron sputtering process, and the specific steps are as follows: Pretreatment of aluminum-lithium alloy particles: Screen out impurities from vacuum-stored aluminum-lithium alloy particles in a protective atmosphere, and select aluminum-lithium alloy particles with a particle size of 20-50 μm; Sputtering film formation: The screened aluminum-lithium alloy particles are placed in a magnetron sputtering device equipped with an aluminum target, and the sputtering parameters are set to coat the aluminum-lithium alloy particles, thereby wrapping a layer of aluminum film on the surface of the aluminum-lithium alloy; Aluminum film passivation treatment: The aluminum-lithium alloy particles wrapped with aluminum film are placed in a constant temperature and humidity phase for passivation treatment to form an oxide film on the outer layer of the aluminum film.

[0028] Sputtering power has an important influence on the density and composition uniformity of aluminum film. Higher sputtering power can increase the number of high-energy electrons bombarding the target, thereby increasing the sputtering yield and deposition rate, and making aluminum atoms deposit more evenly on the substrate. Therefore, when the sputtering power is high, the density of the aluminum film is better and the composition uniformity is higher; with the increase of sputtering power, richer nanostructures will appear on the surface of the aluminum film, and the grain size will become smaller, which will help to improve the coating effect and mechanical properties of the aluminum film. However, when the sputtering power is too high, the deposition rate may not continue to increase linearly; on the one hand, too high sputtering power may lead to too many particles being sputtered, and the mutual collision of particles in space will intensify. Some particles may lose energy due to collision and cannot be effectively deposited on the substrate; on the other hand, too high sputtering power may also cause the "ion implantation effect", that is, the energy of the bombarding ions is largely consumed on the target, resulting in a decrease in the number of particles actually used for deposition, and the deposition rate will decrease instead. In addition, the choice of sputtering pressure will also affect the density and uniformity of the film; and the sputtering time directly determines the thickness of the aluminum film. A longer sputtering time can produce a thicker aluminum film, but too long a sputtering time may increase the internal stress of the film and affect the quality of the film. In fact, in the sputtering process, it is not the role of a single parameter that affects the result. Therefore, in order to obtain an aluminum film that meets the conditions, the sputtering power is set to 1.5~3.5Kw, the pressure is set to 0.3~0.8Mpa, and the sputtering time is 2~8h; the speed of the rolling cylindrical structure is 2-10r / min.

[0029] The temperature, humidity and time of the passivation treatment will directly affect the formation rate, quality, uniformity and final corrosion resistance of the oxide film. Higher temperatures can accelerate the formation rate of the oxide film (passivation film), but too high a temperature may cause the oxide film to be too thick or uneven, or even loose, porous and easy to fall off. The time of the passivation treatment determines the growth thickness of the oxide film. A shorter treatment time may not form a sufficiently dense and uniform oxide film, thereby reducing the corrosion resistance. Excessive treatment time may cause the oxide film to be too thick, which not only wastes resources, but also may affect the mechanical properties and aesthetics of the material. Therefore, in the embodiment of the present application, the temperature of the passivation treatment is 55~65°C, the humidity is 72~85%, and the placement time is 20~30h. Preferably, the temperature of the passivation treatment is 60~62°C, the humidity is 75~80%, and the placement time is 22~24h.

[0030] On the basis of the above scheme, as a further preferred scheme, in the preparation method described in the embodiment of the present application, the magnetron sputtering equipment is a rolling cylindrical structure. Since the aluminum-lithium alloy particles are enriched together in a powder state, they are prone to accumulation. In order to solve this problem, in the embodiment of the present application, a plurality of protrusions are provided on the inner wall of the rolling cylindrical structure, and the plurality of protrusions are arranged equidistantly along the axial direction of the drum. During sputtering, the rolling cylindrical structure rotates, driving the aluminum-lithium alloy powder in the furnace to rotate. The aluminum-lithium alloy powder hits the protrusions, which will cause the original accumulation blocks to be broken, achieving a dispersion effect, which is beneficial to the coating of the aluminum target. Preferably, in some embodiments of the present application, the protrusions are continuous gear-shaped protrusions, which can ensure that the powder accumulation blocks are accurately broken.

[0031] As a further preferred solution, in the preparation method described in the embodiment of the present application, during sputtering film formation, the magnetron sputtering equipment is filled with a protective gas, specifically, the protective gas is nitrogen or an inert gas.

[0032] Embodiment 1 like Figure 1 , Figure 3 and Figure 4 As shown, this embodiment provides an aluminum-lithium alloy material, including an aluminum-lithium alloy particle 10 and an aluminum film 20 coated on the surface of the aluminum-lithium alloy particle 10, wherein an oxide film 30 is formed on the surface of the aluminum film 20, and a bonding interface is formed between the aluminum film 20 and the aluminum-lithium alloy particle 10, and an atomic diffusion layer is formed at the bonding interface, and the average grain size of the crystal grains in the aluminum film 10 is 42nm. Among the aluminum-lithium alloy particles, lithium accounts for 10.40wt% and aluminum accounts for 89.60wt%; the aluminum-lithium alloy material is prepared by the following method: Pretreatment of aluminum-lithium alloy particles: screen out impurities from the vacuum-stored aluminum-lithium alloy particles in an inert gas atmosphere, and select aluminum-lithium alloy particles with a particle size of 20 μm; Sputtering film formation: The screened aluminum-lithium alloy particles are placed in a magnetron sputtering device equipped with an aluminum target, and the sputtering parameters are set. The sputtering power is set to 1.5Kw, the pressure is set to 0.8Mpa, and the sputtering time is 8h. The rotating speed of the rolling cylindrical structure is 2r / min, and the aluminum-lithium alloy particles are coated, and a layer of aluminum film is wrapped on the surface of the aluminum-lithium alloy. Aluminum film passivation treatment: The aluminum-lithium alloy particles wrapped with aluminum film are placed in a constant temperature and humidity phase for passivation treatment at a temperature of 55°C and a humidity of 72% for 24 hours to form an oxide film on the outer layer of the aluminum film.

[0033] The effect of aluminum-lithium alloy particles before and after aluminum film coating can be seen in Figure 2 and Figure 3 . Figure 2This is the SEM image of the aluminum-lithium alloy particles in the original powder, which shows metallographic structures such as "grooves" and "channels". Figure 3 This is the SEM image of the aluminum-lithium alloy particles after being coated with aluminum film. It can be seen that the particles are completely coated and the metallographic structure of the original powder does not exist.

[0034] Embodiment 2 This embodiment provides an aluminum-lithium alloy material, including aluminum-lithium alloy particles and an aluminum film coated on the surface of the aluminum-lithium alloy particles, wherein an oxide film is formed on the surface of the aluminum film, a bonding interface is formed between the aluminum film and the aluminum-lithium alloy particles, and an atomic diffusion layer is formed at the bonding interface, and the average grain size of the grains in the aluminum film is 126nm. Among the aluminum-lithium alloy particles, lithium accounts for 10.40wt% and aluminum accounts for 89.60wt%; the aluminum-lithium alloy material is prepared by the following method: Pretreatment of aluminum-lithium alloy particles: screen out impurities from the vacuum-stored aluminum-lithium alloy particles in an inert gas atmosphere, and select aluminum-lithium alloy particles with a particle size of 50 μm; Sputtering film formation: The screened aluminum-lithium alloy particles are placed in a magnetron sputtering device equipped with an aluminum target, and the sputtering parameters are set, the sputtering power is set to 2Kw, the pressure is set to 0.5Mpa, and the sputtering time is 2h; the rotating speed of the rolling cylindrical structure is 2r / min, and the aluminum-lithium alloy particles are coated, and a layer of aluminum film is wrapped on the surface of the aluminum-lithium alloy; Aluminum film passivation treatment: The aluminum-lithium alloy particles wrapped with aluminum film are placed in a constant temperature and humidity phase for passivation treatment at a temperature of 60°C and a humidity of 80% for 24 hours to form an oxide film on the outer layer of the aluminum film.

[0035] Comparative Examples 1-3 According to the method of the above-mentioned embodiment 1, the aluminum target is replaced with iron, silicon, and nickel (corresponding to Examples 1-3), respectively, to obtain aluminum-lithium alloy particles coated with iron, silicon, and nickel, respectively.

[0036] Performance Testing The coating ratio and calorific value of the aluminum-lithium alloy particles and the original powder of the aluminum-lithium alloy particles obtained in the above Examples 1 and 2 and Comparative Examples 1-3 were tested. The calorific value was tested using an oxygen bomb test method. The test results are shown in Table 1.

[0037] Table 1: Calorific value test results of aluminum-lithium alloy particles The results in Table 1 show that the combustion calorific value of the aluminum-lithium alloy particles after coating in Example 1 and Example 2 is basically unaffected, which is more conducive to maintaining the thermodynamic properties of the powder compared to coating with nickel and other metals or organic matter.

[0038] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. An aluminum-lithium alloy material, characterized in that: It includes aluminum-lithium alloy particles and an aluminum film coated on the surface of the aluminum-lithium alloy particles, an oxide film is formed on the surface of the aluminum film, a bonding interface is formed between the aluminum film and the aluminum-lithium alloy particles, an atomic diffusion layer is formed at the bonding interface, the average particle size of the grains in the aluminum film is 42~126nm; in the atomic diffusion layer, the proportion of aluminum element is 91.2wt%~98.7wt%; the thickness of the aluminum film is 0.3~0.8μm, and the thickness of the oxide film is 0.05~0.15μm.

2. The aluminum-lithium alloy material according to claim 1, characterized in that: The thickness of the atomic diffusion layer is 120-200 nm.

3. A method for preparing the aluminum-lithium alloy material according to claim 1 or 2, characterized in that: The aluminum film is formed on the surface of the aluminum-lithium alloy particles by magnetron sputtering process. The specific steps are as follows: Pretreatment of aluminum-lithium alloy particles: Screening out impurities from vacuum-stored aluminum-lithium alloy particles in a protective atmosphere; Sputtering film formation: The screened aluminum-lithium alloy particles are placed in a magnetron sputtering device equipped with an aluminum target, and the sputtering parameters are set to coat the aluminum-lithium alloy particles, thereby wrapping a layer of aluminum film on the surface of the aluminum-lithium alloy; Aluminum film passivation treatment: The aluminum-lithium alloy particles wrapped with aluminum film are placed in a constant temperature and humidity phase for passivation treatment to form an oxide film on the outer layer of the aluminum film.

4. The preparation method according to claim 3, characterized in that: The size of the aluminum-lithium alloy particles is 20-50 μm.

5. The preparation method according to claim 3, characterized in that: The magnetron sputtering device is a rolling cylindrical structure, and a plurality of protrusions are arranged on the inner wall of the rolling cylindrical structure, and the plurality of protrusions are arranged equidistantly along the axial direction of the drum.

6. The preparation method according to claim 5, characterized in that: During sputtering film formation, the magnetron sputtering equipment is filled with protective gas, the sputtering power is set to 1.5~3.5Kw, the pressure is set to 0.3~0.8Mpa, and the sputtering time is 2~8h; The rotating speed of the rolling cylindrical structure is 2r / min.

7. The preparation method according to claim 5, characterized in that: During the passivation treatment of the aluminum film, the temperature is 55~65℃, the humidity is 72~85%, and the placement time is 20~30h.

8. Use of the aluminum-lithium alloy material as claimed in claim 1 or 2 in the preparation of metal fuel.

Citation Information

Cited By

  • Metal powder magnetron sputtering continuous coating device and method

    CN122484705A