Polyester and preparation method thereof
By performing high-temperature treatment and separation during the cleaning and screening process of polyester bottles, combined with the use of diol depolymerization and catalysts, the problem of difficult removal of nylon high-barrier materials is solved, and low nitrogen content, high color and Repolymerized polyester with heat resistance, suitable for high-quality polyester products in the clothing field.
Patent Information
- Application Number
- CN202310606809.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively remove nylon-based high barrier materials in recycled polyester beverage bottles, resulting in poor color and heat resistance of repolymerized polyester, limiting its application in the field of clothing.
The high-temperature treatment was carried out during the cleaning and screening process of polyester bottles. The yellowed nylon high-barrier materials were separated by color screening and optical screening systems. Then, the depolymerization and polymerization reaction were carried out in the presence of diol, and the high-temperature treatment temperature was controlled. 100-280°C, the time is between 10-300 minutes, the treatment is performed with an inert gas to avoid thermal oxidation and degradation, and a diethylene glycol inhibitor and a catalyst are added to optimize the depolymerization and repolymerization process.
The nitrogen content in the recovered polyester is reduced, and the color tone and heat resistance of the repolymerized polyester is improved, so that polyester products such as fibers have excellent color tone and strength, which is suitable for applications in the clothing field.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to polyester and a preparation method thereof, and in particular to polyester with low nitrogen content prepared by taking recycled polyester as raw material and a preparation method thereof. Background Art
[0002] Polyester (PET) is one of the most commonly used polymers. However, since PET is not biodegradable, its recycling has become a major concern for environmental protection. The sources of recycled PET in my country are mainly divided into the following three categories: waste polyester beverage bottles, waste polyester packaging films, polyester waste yarn and waste textiles. Among them, waste polyester beverage bottles account for more than 60%.
[0003] At present, the recycling of waste polyester beverage bottles is mainly divided into two categories: physical method and chemical method. The physical method is the main method used in China at this stage. The physical method includes crushing, cleaning, screening, and granulating the recycled polyester bottles for direct spinning, which is mainly used in the field of polyester staple fibers. Some high-quality recycled polyester chips can also be used for polyester long fibers. Although the physical method can recycle and reuse polyester beverage bottles at low cost and high efficiency, the recycled polyester beverage bottles are inevitably mixed with sand, dust, other material polymers, etc., and thermal degradation is prone to occur during the processing process, resulting in a decrease in viscosity. For some fields with high requirements for polyester quality, it is difficult to meet actual needs. It is still very difficult to achieve the replacement of virgin polyester with recycled polyester beverage bottles.
[0004] The chemical method is to depolymerize waste polyester beverage bottle flakes into small molecules, such as terephthalic acid (TPA), dimethyl terephthalate (DMT), ethylene glycol terephthalate (BHET), and ethylene glycol (EG). These small molecules can be repolymerized as polyester raw materials after purification, and theoretically, recycled polyester comparable to virgin polyester can be obtained. However, due to the complexity of the composition of waste polyester materials, there are many by-products of the depolymerization products, and the incomplete depolymerization process will also lead to incomplete depolymerization, affecting the subsequent purification process, resulting in the final polyester product quality not meeting the standards. Although some polyester manufacturers have now achieved the industrialization of the chemical method, there are still some urgent problems to be solved in terms of polymer quality control, comprehensive cost, and environmental protection.
[0005] Chinese patent CN115232298A discloses a method for preparing regenerated cationic dyeable polyester chips from waste polyester materials. This method realizes short-process and efficient polyester recycling and gives the recycled polyester cationic dyeability. Chinese patent CN112608514A discloses a method for preparing normal pressure dyeable polyester and producing ultrafine fibers from polyester recycled materials. This method also realizes the normal pressure dyeability of recycled polyester and can prepare ultrafine fibers. Although the above method realizes the functional improvement of recycled polyester, due to the lack of high requirements on the quality of recycled raw materials, a small amount of impurities remain in the recycled polyester raw materials, causing the final product to be severely yellowed, making it difficult to carry out large-scale application in clothing applications. Summary of the invention
[0006] The object of the present invention is to provide a polyester prepared from recycled polyester as a raw material and a preparation method thereof, wherein the obtained polyester has a low nitrogen content and has good color tone and heat resistance.
[0007] The technical solution of the present invention is as follows: The polyester is obtained by depolymerizing and then polymerizing the recycled polyester, wherein the nitrogen content of the polyester is below 10000 ppm, preferably below 1000 ppm, and more preferably below 100 ppm.
[0008] The present invention also discloses a method for preparing the above-mentioned polyester, which takes recycled polyester bottle flakes as raw materials, performs high-temperature treatment at any stage of the cleaning and screening process of the polyester bottle flakes, then separates the yellowed bottle flakes through a screening system, depolymerizes the remaining bottle flakes in the presence of diol, transfers them to a polymerization kettle after the depolymerization is completed, then vacuumizes and heats to start a polymerization reaction, and spits out the polyester after the polymerization reaction is completed.
[0009] The nitrogen content in the recycled polyester bottle flakes is preferably below 10,000 ppm.
[0010] The temperature of the high temperature treatment is preferably 100 to 280° C., and the time of the high temperature treatment is preferably 10 to 300 minutes.
[0011] The invention treats the recycled polyester, screens and removes yellowing impurities, and then performs alcoholysis and polymerization to obtain the polyester. The polyester has a low nitrogen content and good color tone and heat resistance. DETAILED DESCRIPTION
[0012] The main component of polyester bottle flakes is polyethylene terephthalate. This type of polyester is easy to recycle and depolymerize, and is widely used. Regarding the chemical recycling method of polyester beverage bottles, one of them is to depolymerize the recycled polyester into single molecules or oligomers, and then polymerize it to obtain polyester. Through this method, various additives can be added to the depolymerization product, so that the obtained polyester has diversity. At the same time, this method has the advantages of simple production process and small equipment investment.
[0013] However, since recycled polyester often contains impurities such as dyes, pigments, nylon, polyethylene, polypropylene, polyvinyl alcohol, etc., the by-products produced by thermal cracking during the depolymerization process will cause the color tone and heat resistance of the re-polymerized polyester to be poor, all of which will limit its widespread application in the polyester industry.
[0014] In order to improve the performance of repolymerized polyester, inorganic impurities such as dust and sand, and organic impurities such as glue, polypropylene, and polyethylene are usually removed during the cleaning stage. Then, during the screening stage, bottle flakes containing dyes and pigments are removed through color screening and optical screening systems. This ensures the quality of the polyester obtained from the alcoholysis and repolymerization of polyester bottle flakes to the greatest extent possible.
[0015] However, in recent years, as the public's demand for flavored beverages has gradually increased, in order to ensure the taste of the beverages, more multi-layer polyester packaging bottles have appeared on the market. The interlayers in the multi-layer polyester packaging bottles are mostly made of nylon-based high-barrier materials, which can prevent the diffusion of carbon dioxide gas and the like, ensuring the taste of the beverage. However, nylon-based high-barrier materials are difficult to be effectively separated in the recycling of polyester beverage bottles, mainly because nylon-based high-barrier materials have extremely similar physical and chemical properties to polyester, and it is difficult to achieve effective separation of the two, whether through physical washing, color screening, optical screening, etc. In the depolymerization and repolymerization process of chemical recycling, these nylon-based high-barrier materials will decompose and color, which seriously affects the quality of the repolymerized polyester and limits its application in the field of clothing.
[0016] The present invention provides a method for effectively separating nylon high barrier materials from polyester materials in recycled polyester bottle flakes, so that the remaining polyester materials can be alcoholyzed and then polymerized to obtain repolymerized polyester with low nitrogen content. Only when the nitrogen content in the repolymerized polyester is below 10000 ppm, can the repolymerized polyester have good color tone and heat resistance, and the color tone and strength of polyester products such as fibers are excellent. In order to further improve the color tone and heat resistance of the repolymerized polyester, the present invention preferably has a nitrogen content of less than 1000 ppm in the repolymerized polyester, and more preferably less than 100 ppm.
[0017] The nylon-based high barrier material is generally one or more of nylon 6, nylon 66, nylon 56, MXD6, etc. If these nylon-based high barrier materials are not separated before alcoholysis, it will have an adverse effect on the physical properties of the final repolymerized polyester and its subsequent products.
[0018] The specific method of effectively separating nylon high barrier materials from polyester materials is to perform high temperature treatment at any stage of the cleaning and screening process of polyester bottle flakes. After being treated at high temperature for a certain period of time, nylon high barrier materials will turn yellow, turning into yellow or brown, and then the yellowed bottle flakes are separated by screening systems such as color sorting systems and optical sorting systems, thereby obtaining polyester bottle flakes with lower impurity content.
[0019] When the treatment temperature of the high temperature treatment is too low, the nylon high barrier material changes color very slowly and the color change is not obvious, the separation efficiency is low, and it is difficult to meet the production needs; when the treatment temperature of the high temperature treatment is too high, especially when it exceeds the melting point of polyester, the polyester bottle flakes will melt, the shape will change significantly, and even agglomerate, making it difficult to separate later. Therefore, the present invention preferably uses a temperature of 100 to 280°C, more preferably 100 to 260°C, and most preferably 150 to 240°C.
[0020] The time of the high temperature treatment also affects the separation effect. If the time is too short, the nylon high barrier material will not change color obviously, and it is difficult to achieve effective separation; if the time is too long, although the nylon high barrier material can be fully discolored, which is convenient for later screening and separation, it will lead to low production efficiency and difficulty in large-scale application. Therefore, the present invention preferably uses a high temperature treatment time of 10 to 300 minutes, and more preferably 30 to 150 minutes.
[0021] The high temperature treatment can be carried out in air, inert gas or vacuum. Since air contains oxygen, although it can accelerate the discoloration of nylon high barrier materials and improve separation efficiency, it will also cause the polyester bottle flakes to discolor or thermal oxidation degradation during the high temperature treatment, resulting in a low yield of polyester bottle flakes during later separation, and the color tone of the polyester obtained after the depolymerization and repolymerization of the thermal oxidation degraded polyester bottle flakes deteriorates. Therefore, the high temperature treatment is preferably carried out in an inert gas or vacuum, and the inert gas can be nitrogen, argon, helium, etc.
[0022] By removing dust, sand, glue, polypropylene, polyethylene and other impurities through conventional separation means, and removing nylon high barrier materials through special means of high temperature treatment and re-separation, the nitrogen content in the obtained polyester bottle flakes can reach below 10,000 ppm, thereby obtaining repolymerized polyester with a nitrogen content of less than 10,000 ppm.
[0023] After the separation process is completed, the remaining polyester bottle flakes are depolymerized in the presence of diols. After the depolymerization is completed, a catalyst and / or copolymerization component is added, and then the vacuum is evacuated and the temperature is raised to start the polymerization reaction. After the polymerization reaction is completed, the polyester is spit out to obtain the polyester.
[0024] The depolymerization temperature of polyester bottle flakes is 150-260℃, under pressure or normal pressure. If the depolymerization temperature is too low, the depolymerization efficiency is low and it is difficult to meet production needs. If the depolymerization temperature is too high, although the depolymerization can be completed in a short time, the depolymerization pressure is high, the equipment load is large, and the production safety is reduced.
[0025] During depolymerization, diol needs to be added as a depolymerizing agent, mainly to utilize diol to destroy the macromolecular chain, reduce the molecular weight of polyester, and improve fluidity. Due to the high temperature and high molar ratio of alcohol and acid during the depolymerization process, if it is not controlled, a large amount of diethylene glycol will be produced, and diethylene glycol will also affect the heat resistance of the repolymerized polyester. If the diethylene glycol content is high, the regularity of the repolymerized polyester will deteriorate, and the creep irreversible part of polyester products such as fibers in the later stage will increase, and the shrinkage rate of the fibers will increase, affecting the application of the fibers in clothing. The diethylene glycol content in the esterified liquid after depolymerization described in the present invention is 0.5-2.0wt%.
[0026] In order to inhibit the formation of diethylene glycol, a diethylene glycol inhibitor may be added during the depolymerization process. The diethylene glycol inhibitor includes, but is not limited to, one or more of lithium acetate, sodium acetate, potassium acetate, lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium hydroxide, potassium hydroxide, sodium hydroxide, cesium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrabutylammonium hydroxide.
[0027] After the depolymerization is completed, the depolymerization liquid is transferred to an auxiliary agent adding kettle or a polymerization kettle. Since the recovered polyester contains a polymerization catalyst, repolymerization can be achieved without adding a catalyst. In addition, in order to further improve the polymerization activity, a polymerization catalyst such as an antimony catalyst, a titanium catalyst, a germanium catalyst or an aluminum catalyst can be added to the depolymerization liquid, such as antimony trioxide, antimony glycol, antimony acetate, germanium oxide, germanium acetate, tetrabutyl titanate, tetraisopropyl titanate, titanium glycol, aluminum glycol, TYZOR® ACtivate™ 422, TYZOR® ACtivate™ 436, TOYOBO GS Catalyst®, etc. In addition, in order to achieve the diversification of recycled polyester, various additives and copolymer components can be added, the additives include but are not limited to titanium dioxide, zinc oxide, calcium oxide, magnesium oxide, zirconium oxide, copper oxide, titanium nitride, etc.; the copolymer components include but are not limited to polyethylene glycol, cyclohexanedicarboxylic acid and its derivatives, cyclohexanedimethanol, sodium 3,5-dicarboxybenzenesulfonate and its derivatives, adipic acid and its derivatives, sodium 3-carboxybenzenesulfonate and its derivatives, isophthalic acid, sebacic acid, etc.
[0028] The polyester obtained by repolymerizing the recycled polyester of the present invention has the advantages of low nitrogen content, excellent color tone, good heat resistance and good spinnability.
[0029] The present invention is described in more detail below by way of examples. The physical properties parameters involved in the examples are measured by the following methods.
[0030] (1) Test of N content Weigh 15-20 mg of sample, place the sample in oxygen flow and burn it, use oxidant to fully oxidize its organic components, and quantitatively convert N element into its corresponding volatile oxide, let these products flow through silica gel column chromatography, use thermal conductivity cell detector to measure their concentrations respectively, and finally use external standard method to determine the content of N element. The final result is the average value of 5 tests.
[0031] (2) Heat resistance evaluation method Weigh 8g of slices and put them into a test tube. Heat them at 300℃ under nitrogen for 3 hours. Test the carboxyl content of the slices before and after the heating treatment. The larger the carboxyl content ΔCOOH (COOH before heating treatment - COOH after heating treatment) before and after the heating treatment, the worse the heat resistance of the polyester. The final result is the average value of 5 tests.
[0032] (3) Hue test Use a colorimeter (SM-T45) manufactured by SUGA Testing Instrument Co., Ltd. to calibrate with a standard white plate under C2 light source. After calibration, place the slices in a special glass container and test the slice Lab value (L value (brightness index), a value (red / green index), b value (yellow / blue index)). The lower the b value, the better the color tone. The final result is the average of 5 tests.
[0033] Embodiment 01: Purification of recycled polyester bottle flakes: After washing, screening and drying, the recycled polyester beverage bottle flakes are treated in air at 200°C for 120 minutes, and then passed through a color sorting system and an optical screening system to remove the yellowed bottle flakes to obtain high-purity polyester bottle flakes. The nitrogen content in the high-purity polyester bottle flakes is 100ppm.
[0034] Repolymerization of polyester: Put the purified polyester bottle flakes into the depolymerization kettle, add a certain amount of ethylene glycol and diethylene glycol inhibitor lithium acetate, then depolymerize at 230°C to obtain an intermediate, move the intermediate into the polymerization kettle, then add a heat stabilizer, a catalyst antimony trioxide, and an additive titanium dioxide, vacuumize and heat up, and perform a polycondensation reaction at 290°C. When the polymer reaches the required viscosity, it is spit out and pelletized to obtain polyester chips. The specific physical properties of the polyester chips are shown in Table 1.
[0035] Embodiments 02 to 15: The temperature, time and atmosphere of the high temperature treatment were changed. Other conditions were the same as in Example 1. The specific physical properties are shown in Table 1.
[0036] Comparative Example 01: Purification of recycled polyester bottle flakes: After washing, screening and drying, the recycled polyester beverage bottle flakes are purified to obtain purified polyester bottle flakes, in which the nitrogen content is 12000ppm.
[0037] Repolymerized polyester: The preparation process is the same as in Example 1.
[0038] Since the recycled polyester bottle flakes are not subjected to high-temperature treatment, some beverage bottle flakes formed by nylon-based high-barrier materials still remain in the purified polyester bottle flakes. The polyester after depolymerization and repolymerization has a high N element content, poor color tone and low heat resistance.
[0039]
Claims
1. Polyester, obtained by depolymerizing and then polymerizing recycled polyester, characterized in that: The nitrogen content in the polyester is below 10000 ppm.
2. The polyester according to claim 1, characterized in that: The nitrogen content in the polyester is below 1000 ppm.
3. The polyester according to claim 1 or 2, characterized in that: The nitrogen content in the polyester is below 100 ppm.
4. The method for preparing the polyester according to claim 1, characterized in that: Recycled polyester bottle flakes are used as raw materials. At any stage of the cleaning and screening process of the polyester bottle flakes, high-temperature treatment is carried out, and then the yellowed bottle flakes are separated through a screening system. The remaining bottle flakes are depolymerized in the presence of diols. After the depolymerization is completed, they are transferred to a polymerization kettle, and then vacuum is evacuated and the temperature is raised to start the polymerization reaction. After the polymerization reaction is completed, polyester is spit out to obtain polyester.
5. The method for preparing polyester according to claim 4, characterized in that: The nitrogen content in the recycled polyester bottle flakes is below 10000 ppm.
6. The method for preparing polyester according to claim 4 or 5, characterized in that: The temperature of the high temperature treatment is 100-280°C.
7. The method for preparing polyester according to claim 4 or 5, characterized in that: The high temperature treatment time is 10 to 300 minutes.
8. The method for preparing polyester according to claim 4 or 5, characterized in that: The high temperature treatment is performed in an inert gas or in a vacuum.