Polymer-induced rhodamine 6G film fluorescence enhancement method
By using cellulose nanocrystals and polymer assembly technology in rhodamine 6G films, a chiral nematic structure was formed, which solved the problem of rhodamine 6G self-quenching, achieved a significant improvement in fluorescence performance, and provided a simple and efficient fluorescence enhancement method.
Patent Information
- Application Number
- CN202411373257.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-26
AI Technical Summary
Rhodamine 6G is troubled by self-quenching problems in photochemical applications. The preparation process of the prior art methods is complex and the fluorescence enhancement effect is limited. A simple and efficient method is needed to improve its fluorescence performance.
By preparing an aqueous dispersion of cellulose nanocrystals, adding polymer and rhodamine 6G solution, stirring evenly, pouring it into a Petri dish to dry it into a film, forming a rhodamine 6G film with chiral nematic structure, using polymer as dispersion The medium reduces the molecular aggregation of rhodamine 6G and improves fluorescence luminescence.
The fluorescence of rhodamine 6G is significantly enhanced, the preparation method is simple, and it has rich polymer selectivity. It is suitable for different situations, reducing fluorescence quenching and improving fluorescence luminescence performance.
Smart Images

Figure CN119019724A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorescence enhancement, and particularly relates to a method for polymer-induced fluorescence enhancement of a rhodamine 6G film. Background Art
[0002] Rhodamine 6G is a commonly used environmentally friendly organic water-soluble cationic fluorescent dye with a rigid planar structure. It easily absorbs the energy of incident light and emits long waves, thereby generating fluorescence. It has a high fluorescence quantum yield and is widely used for fluorescence labeling or quantitative analysis, especially in biophotonic research, spectroscopy and laser science. However, due to the limitations of the fluorescence properties and intensity of Rhodamine 6G itself, in some photochemical applications, Rhodamine 6G is often plagued by problems such as self-quenching, resulting in huge challenges in its application and promotion. Therefore, modifying Rhodamine 6G to improve its fluorescence properties is an effective way to expand Rhodamine 6G.
[0003] [Lin et al. Journal of Photochemistry & Photobiology, A: Chemistry 2021, 406, 112992] reported a method for enhancing the fluorescence of Rhodamine 6G by photoinitiating monomer polymerization. This method uses HPMA as a monomer and Rhodamine 6G as a photoinitiator. HPMA monomers are polymerized into polymer chains by illumination, and further assembled into micelles or vesicles, and Rhodamine 6G is encapsulated in micelles or vesicles to reduce its quenching and increase fluorescence. The fluorescence of Rhodamine 6G was enhanced by about 2.5 times. However, the preparation process of this method is complicated and the fluorescence enhancement effect is limited. It is very necessary to develop a method for enhancing the fluorescence of Rhodamine 6G that is effective, simple and efficient. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for polymer-induced fluorescence enhancement of rhodamine 6G thin films, by preparing an aqueous dispersion of CNC, adding a polymer and a rhodamine 6G aqueous solution to the dispersion, stirring the mixture evenly at room temperature, pouring the mixture into a culture dish, drying to form a film, and preparing a series of rhodamine 6G thin films with different properties. The present invention has the advantages of simple preparation method, significant enhancement effect, and chiral nematic structure.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0007] Step 1, preparing an aqueous dispersion of cellulose nanocrystals;
[0008] Step 2, adding a polymer to the dispersion to obtain a mixed solution;
[0009] Step 3, adding the rhodamine 6G solution to the mixed solution and stirring;
[0010] Step 4, pour the mixed solution into a culture dish and dry it into a film.
[0011] In one embodiment, the aqueous dispersion of cellulose nanocrystals is prepared by hydrolyzing cotton pulp with concentrated sulfuric acid.
[0012] In one embodiment, the polymer is one or more of polyethylene glycol 200, polyethylene glycol 2000, polyethylene glycol 20000, polyvinyl alcohol, and polyvinyl pyrrolidone.
[0013] In one embodiment, the mass fraction of the aqueous dispersion of cellulose nanocrystals is 3-4%.
[0014] In one embodiment, the mass fraction of the polymer used in the mixed solution is 5%, the volume ratio of the cellulose dispersion to the polymer is 1.8-32, the mass fraction of the rhodamine 6G solution is 0.05-0.1%, and the volume ratio of the rhodamine 6G solution to the mixed solution is 0.02-0.3.
[0015] In one embodiment, the mass fraction of rhodamine 6G in the obtained film is 0.1-0.5%, and the mass fraction of the polymer is 5%-40%.
[0016] In one embodiment, the drying film forming process is performed at room temperature.
[0017] The composite film obtained by the method for enhancing the fluorescence of the rhodamine 6G film induced by the polymer has a chiral nematic structure.
[0018] In one embodiment, the composite film has cellulose nanocrystals as the main body, rhodamine 6G and polymer as the objects, rhodamine 6G as the luminescent substance, and the polymer as the dispersion medium, which reduces the molecular aggregation of rhodamine 6G in the composite film, thereby reducing fluorescence quenching and improving fluorescence luminescence.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The preparation method of the Rhodamine 6G composite film is simple and has a significant fluorescence enhancement effect. At the same time, the composite film has a chiral nematic structure. In addition, there are a variety of polymers to choose from, which can be applied to different situations. The polymer is adsorbed on the surface of cellulose nanocrystals through physical and chemical effects, reducing the electrostatic attraction between positively charged Rhodamine 6G and negatively charged cellulose nanocrystals, reducing the fluorescence quenching caused by the aggregation of Rhodamine 6G molecules in the composite film, and achieving fluorescence enhancement. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a relationship diagram between the ratio of the fluorescence intensity of the CNC / PEG200 / Rh6G film with a polymer PEG200 content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without the polymer and the polymer content.
[0022] Figure 2 It is a relationship diagram between the ratio of the fluorescence intensity of the CNC / PEG2000 / Rh6G film with a polymer PEG2000 content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without the polymer and the polymer content.
[0023] Figure 3 It is a relationship diagram between the ratio of the fluorescence intensity of the CNC / PEG20000 / Rh6G film with a polymer PEG20000 content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without the polymer and the polymer content.
[0024] Figure 4 It is a relationship diagram between the ratio of the fluorescence intensity of the CNC / PVA / Rh6G film with a polymer PVA content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without a polymer and the polymer content.
[0025] Figure 5 It is a relationship diagram between the ratio of the fluorescence intensity of the CNC / PVP / Rh6G film with a polymer PVP content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without a polymer and the polymer content. DETAILED DESCRIPTION
[0026] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.
[0027] The present invention is a method for polymer-induced fluorescence enhancement of rhodamine 6G thin films, wherein cellulose nanocrystals are used as the main body, rhodamine 6G and polymers are used as the guest for host-guest assembly preparation, wherein rhodamine 6G is used as the luminescent substance and the polymer is used as the dispersion medium, and the molecular aggregation of rhodamine 6G in the composite film is reduced, thereby reducing fluorescence quenching and improving fluorescence luminescence. The specific steps can be described as follows:
[0028] Step 1, preparing an aqueous dispersion of cellulose nanocrystals.
[0029] In this step, concentrated sulfuric acid can be used to hydrolyze cotton pulp to prepare an aqueous dispersion of cellulose nanocrystals. The preparation method can be further described as follows:
[0030] First, tear the cotton pulp board into small pieces, break it in a pulper, and then tear it into small balls, dry it in a 30℃ oven for later use. Add 20g of cotton pulp to 200mL, 64wt% H2SO4, stir at 55℃ for 90min, and after the reaction is completed, add a large amount of water to stop the reaction. Let the obtained white suspension stand overnight, pour out the supernatant, centrifuge the lower suspension at 8000rmp / min for 6min, pour out the supernatant, wash it with deionized water and centrifuge it again, and repeat the centrifugation three times. Pour the centrifuged CNC into the ultrafiltration cup, add water and pressure ultrafiltration until the pH of the filtrate stabilizes at around 3.
[0031] Finally, the ultrafiltered CNC can be taken out and diluted to a mass concentration of 3-4% for later use.
[0032] Step 2: adding a polymer to the dispersion to obtain a mixed solution.
[0033] In this step, the polymer is added to the dispersion, so that the polymer can be adsorbed on the surface of the cellulose nanocrystals through physical and chemical effects.
[0034] The polymer may be one or more of polyethylene glycol 200, polyethylene glycol 2000, polyethylene glycol 20000, polyvinyl alcohol, and polyvinyl pyrrolidone. The mass fraction of the polymer used in the mixed solution is 5%, and the volume ratio of the cellulose dispersion to the polymer is 1.8-32.
[0035] Step 3, adding the rhodamine 6G solution into the mixed solution and stirring.
[0036] In this step, the Rhodamine 6G solution and the mixed solution are stirred to make them uniformly mixed, wherein the mass fraction of the Rhodamine 6G solution is 0.05-0.1%, and the volume ratio of the Rhodamine 6G solution to the mixed solution is 0.02-0.3.
[0037] Step 4, pouring the mixed solution into a culture dish and drying it to form a film, wherein the obtained film has a chiral nematic structure, wherein the mass fraction of rhodamine 6G is 0.1-0.5%, and the mass fraction of the polymer is 5%-40%.
[0038] The present invention can achieve the regulation of polymer content in the composite film by adding polymers with fixed mass fraction and different volumes. The mass fraction of rhodamine 6G in the obtained film is 0.1-0.5%, and the mass fraction of the polymer is 5%-40%.
[0039] Each step of the present invention can be carried out at room temperature.
[0040] The preparation method of the present invention can be applied to improving the fluorescence performance of rhodamine 6G by polymers of the same type but with different molecular weights and concentrations, and can also be applied to improving the fluorescence performance of rhodamine 6G by polymers of different types.
[0041] The invention has the advantages of simple preparation method, significant performance improvement and chiral nematic structure, and has potential application in the field of fluorescent probes.
[0042] The following are several specific embodiments of the present invention.
[0043] Example 1
[0044] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0045] Step 1, hydrolyzing cotton pulp with concentrated sulfuric acid to obtain a 3wt% CNC aqueous dispersion.
[0046] Step 2, at room temperature, add 0 mL, 0.047 mL, 0.1 mL, 0.225 mL, 0.386 mL, and 0.6 mL of 5% PEG200 aqueous solution to 1.5 mL of the dispersion obtained in step 1, respectively, and stir at room temperature for 60 min to obtain a mixed solution.
[0047] Step 3: add 0.225 mL of 0.1 wt% Rh6G aqueous solution into each mixed solution of step 2 and stir for 60 min.
[0048] Step 4, pouring the mixed solutions of various specifications obtained in step 3 into a culture dish at room temperature, drying them into films at room temperature, and obtaining CNC / PEG200 / Rh6G composite films with PEG200 contents of 0%, 5%, 10%, 20%, 30%, and 40%, respectively.
[0049] Example 2
[0050] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0051] Step 1, hydrolyzing cotton pulp with concentrated sulfuric acid to obtain a 3wt% CNC aqueous dispersion.
[0052] Step 2, at room temperature, add 0 mL, 0.047 mL, 0.1 mL, 0.225 mL, 0.386 mL, and 0.6 mL of 5% PEG2000 aqueous solution to 1.5 mL of the dispersion obtained in step 1, respectively, and stir at room temperature for 60 min to obtain a mixed solution.
[0053] Step 3: add 0.225 mL of 0.1 wt% Rh6G aqueous solution into each mixed solution of step 2 and stir for 60 min.
[0054] Step 4, pouring the mixed solutions of various specifications obtained in step 3 into a culture dish at room temperature, drying them into films at room temperature, and obtaining CNC / PEG2000 / Rh6G composite films with PEG2000 contents of 0%, 5%, 10%, 20%, 30%, and 40%, respectively.
[0055] Example 3
[0056] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0057] Step 1, hydrolyzing cotton pulp with concentrated sulfuric acid to obtain a 3wt% CNC aqueous dispersion.
[0058] Step 2, at room temperature, add 0 mL, 0.047 mL, 0.1 mL, 0.225 mL, 0.386 mL, and 0.6 mL of a 5% PEG20000 aqueous solution to 1.5 mL of the dispersion obtained in step 1, respectively, and stir at room temperature for 60 min to obtain a mixed solution.
[0059] Step 3: add 0.225 mL of 0.1 wt% Rh6G aqueous solution into each mixed solution of step 2 and stir for 60 min.
[0060] Step 4, pour the mixed solutions of various specifications obtained in step 3 into a culture dish at room temperature, dry them into films at room temperature, and obtain CNC / PEG20000 / Rh6G composite films with PEG20000 contents of 0%, 5%, 10%, 20%, 30%, and 40%, respectively.
[0061] Example 4
[0062] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0063] Step 1, hydrolyzing cotton pulp with concentrated sulfuric acid to obtain a 3wt% CNC aqueous dispersion.
[0064] Step 2, at room temperature, add 0 mL, 0.047 mL, 0.1 mL, 0.225 mL, 0.386 mL, and 0.6 mL of 5% PVA aqueous solution to 1.5 mL of the dispersion obtained in step 1, respectively, and stir at room temperature for 60 min to obtain a mixed solution.
[0065] Step 3: add 0.225 mL of 0.1 wt% Rh6G aqueous solution into each mixed solution of step 2 and stir for 60 min.
[0066] Step 4, pour the mixed solutions of various specifications obtained in step 3 into a culture dish at room temperature, dry them into films at room temperature, and obtain CNC / PVA / Rh6G composite films with PVA contents of 0%, 5%, 10%, 20%, 30%, and 40%, respectively.
[0067] Example 5
[0068] A method for polymer-induced fluorescence enhancement of rhodamine 6G film comprises the following steps:
[0069] Step 1, hydrolyzing cotton pulp with concentrated sulfuric acid to obtain a 4 wt% CNC aqueous dispersion.
[0070] Step 2, at room temperature, add 0 mL, 0.063 mL, 0.13 mL, 0.3 mL, 0.514 mL, and 0.8 mL of 5% PVP aqueous solution to 1.5 mL of the dispersion obtained in step 1, respectively, and stir at room temperature for 60 min to obtain a mixed solution.
[0071] Step 3: add 0.225 mL of 0.1 wt% Rh6G aqueous solution into the mixed solutions of various specifications in step 2 in sequence and stir for 60 min.
[0072] Step 4, pouring the mixed solutions of various specifications obtained in step 3 into culture dishes at room temperature, drying them into films at room temperature, and obtaining CNC / PVP / Rh6G composite films with PVP contents of 0%, 5%, 10%, 20%, 30%, and 40%, respectively.
[0073] The present invention has confirmed the successful enhancement of the fluorescence performance of the Rhodamine 6G film induced by the polymer through fluorescence luminescence image characterization. Figure 1 to Figure 5 shown.
[0074] Figure 1 The figure is a ratio of the fluorescence intensity of the CNC / PEG200 / Rh6G film with a polymer PEG200 content of 0%-40% to the fluorescence intensity of the CNC / Rh6G film without the polymer. It can be seen that as the content of the polymer PEG200 increases from 5% to 40%, the ratio of its fluorescence intensity to the fluorescence intensity of the CNC / Rh6G film without the polymer gradually increases.
[0075] Figure 2 The figure is a ratio diagram of the fluorescence intensity of the CNC / PEG2000 / Rh6G film with a polymer PEG2000 content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without polymer. It can be seen that with the increase of the polymer PEG2000 content, from 5% to 40%, the ratio of its fluorescence intensity to the fluorescence intensity of the CNC / Rh6G film without polymer gradually increases, and the ratio reaches a peak when the polymer PEG2000 content is 30%, and then decreases.
[0076] Figure 3 The figure is a ratio diagram of the fluorescence intensity of the CNC / PEG20000 / Rh6G film with a polymer PEG20000 content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without polymer. It can be seen that with the increase of the polymer PEG20000 content, from 5% to 40%, the ratio of its fluorescence intensity to the fluorescence intensity of the CNC / Rh6G film without polymer gradually increases, and the ratio reaches a peak when the polymer PEG20000 content is 20%, and then decreases.
[0077] Figure 4 This is a ratio diagram of the fluorescence intensity of the CNC / PVA / Rh6G film with a polymer PVA content of 0%-40% and the fluorescence intensity of the CNC / Rh6G film without a polymer. It can be seen that as the polymer PVA content increases from 5% to 40%, the ratio of its fluorescence intensity to the fluorescence intensity of the CNC / Rh6G film without a polymer gradually increases.
[0078] Figure 5 It is a ratio diagram of the fluorescence intensity of CNC / PVP / Rh6G film with a polymer PVP content of 0%-40% and the fluorescence intensity of CNC / Rh6G film without polymer. It can be seen that with the increase of polymer PVP content, from 5% to 40%, the ratio of its fluorescence intensity to the fluorescence intensity of CNC / Rh6G film without polymer gradually increases, and the ratio reaches a peak when the polymer PVP content is 30%, and then decreases.
[0079] According to the above examples, it can be seen that, through the described implementation steps, polymers of different types and concentrations can successfully induce changes in the fluorescence properties of the Rhodamine 6G film, which proves the effectiveness of the method of polymer-induced fluorescence enhancement of the Rhodamine 6G film proposed in the present invention.
Claims
1. A method for polymer-induced fluorescence enhancement of rhodamine 6G film, characterized in that: The steps include: Step 1, preparing an aqueous dispersion of cellulose nanocrystals; Step 2, adding a polymer to the dispersion to obtain a mixed solution; Step 3, adding the rhodamine 6G solution to the mixed solution and stirring; Step 4, pour the mixed solution into a culture dish and dry it into a film.
2. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 1, characterized in that: The aqueous dispersion of cellulose nanocrystals is prepared by hydrolyzing cotton pulp with concentrated sulfuric acid.
3. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 1, characterized in that: The polymer is one or more of polyethylene glycol 200, polyethylene glycol 2000, polyethylene glycol 20000, polyvinyl alcohol, and polyvinyl pyrrolidone.
4. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 1, 2 or 3, characterized in that: The mass fraction of the aqueous dispersion of the cellulose nanocrystals is 3-4%.
5. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 4, characterized in that: The mass fraction of the polymer used in the mixed solution is 5%, the volume ratio of the cellulose dispersion to the polymer is 1.8-32, the mass fraction of the rhodamine 6G solution is 0.05-0.1%, and the volume ratio of the rhodamine 6G solution to the mixed solution is 0.02-0.
3.
6. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 5, characterized in that: The mass fraction of rhodamine 6G in the obtained film is 0.1-0.5%, and the mass fraction of the polymer is 5%-40%.
7. The method for polymer-induced fluorescence enhancement of rhodamine 6G thin film according to claim 1, characterized in that: The drying and film-forming process is carried out at room temperature.
8. A composite film obtained by the method for polymer-induced fluorescence enhancement of Rhodamine 6G film according to claims 1 to 7.
9. The composite film according to claim 8, characterized in that: It has a chiral nematic structure.
10. The composite film according to claim 8, characterized in that: Cellulose nanocrystals are used as the main body, Rhodamine 6G and polymers are used as objects, Rhodamine 6G is used as the luminescent substance, and the polymer is used as the dispersion medium to reduce the molecular aggregation of Rhodamine 6G in the composite film, thereby reducing fluorescence quenching and improving fluorescence luminescence.
Citation Information
Cited By
Carbonized polymer / cellulose nanocrystal composite material for efficient circular polarization luminescence and phosphorescence emission as well as preparation and application of carbonized polymer / cellulose nanocrystal composite material
CN119613817A