Basalt-based shielding material and preparation method thereof
Through the composite materials of basalt fibers, activated carbon fibers and modified graphene, combined with surface modification technology of dopamine and nanosilicon dioxide, a three-dimensional porous structure and conductive network are formed, solving the problem of low performance of existing electromagnetic shielding materials and achieving lightweight High quality and high efficiency electromagnetic shielding performance.
Patent Information
- Application Number
- CN202411211364.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing electromagnetic shielding materials have low effectiveness in blocking electromagnetic radiation and are large in thickness, making it difficult to meet the needs of lightweight, high-strength and high-efficiency electromagnetic shielding.
A composite material of basalt fibers, activated carbon fibers, modified graphene and epoxy resin is used to form a three-dimensional porous structure and conductive network through the surface modification of dopamine and nanosilicon dioxide to enhance the electromagnetic shielding performance of the material.
It realizes lightweight and efficient electromagnetic shielding performance, improves the tensile strength, bending strength and wear resistance of the material, and significantly improves the absorption and reflection ability of electromagnetic waves.
Smart Images

Figure BDA0005020393630000131 
Figure BDA0005020393630000141
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of shielding materials, and in particular to a basalt-based shielding material and a preparation method thereof. Background Art
[0002] With the rapid development of modern information technology, electromagnetic waves have been widely used in electronic products, data transmission, electronic communications, wireless network systems, satellite launches, modern detection technology, radar detection technology, medical diagnosis and other fields, providing great convenience for people's lives while also bringing serious electromagnetic radiation pollution problems. Considering the diversity and inevitability of electromagnetic wave pollution sources, the use of electromagnetic shielding measures is an important and feasible way to control pollution and reduce the hazards of electromagnetic radiation.
[0003] In electromagnetic shielding, reflection and absorption are the main ways to block electromagnetic radiation. For the reflection of electromagnetic radiation, the material must have a movable charge carrier, while the absorption of electromagnetic radiation mainly depends on the interaction between the electric and magnetic dipoles in the radiation and the electromagnetic field. Therefore, the shielding material needs to have a certain conductivity and form a good conductive path. Metal materials are often used in electromagnetic shielding because they have mobile electrons and show high conductivity. However, the shielding effectiveness of metal shielding materials is low and the material thickness is large. Resin-based composite materials have the characteristics of light weight and high strength, but their low conductivity and low electromagnetic interference protection capabilities greatly limit their application. Summary of the invention
[0004] The object of the present invention is to provide a basalt-based shielding material which has light weight, high strength and high efficiency electromagnetic shielding performance.
[0005] Another object of the present invention is to provide a method for preparing a basalt-based shielding material, which can improve the interface bonding strength of each raw material and enhance the electromagnetic shielding performance of the material.
[0006] The embodiments of the present invention are implemented by the following technical solutions:
[0007] A basalt-based shielding material comprises the following raw materials in parts by weight: 10-20 parts of basalt fiber, 1-10 parts of activated carbon fiber, 5-12 parts of modified graphene, 10-20 parts of epoxy resin, 1-5 parts of polymethyl methacrylate microspheres, 1-5 parts of surfactant and 1-5 parts of curing agent.
[0008] A method for preparing a basalt-based shielding material comprises the following steps:
[0009] S1, immersing basalt fiber in dopamine solution for polymerization reaction, washing with water, drying to obtain polydopamine-coated basalt fiber, adding nano-silicon dioxide into buffer solution for ultrasonic treatment, then adding polydopamine-coated basalt fiber, stirring, drying to obtain surface-modified basalt fiber;
[0010] S2, then using a surfactant to prepare an activated carbon fiber dispersion, adding polymethyl methacrylate microspheres to the activated carbon fiber dispersion, mixing, freeze-drying, and heat-treating to obtain a three-dimensional porous carbon fiber;
[0011] S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature, and then cure at 60-65° C. to obtain the basalt-based shielding material.
[0012] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0013] In the present invention, the surface of the activated carbon fiber has more active groups (hydroxyl, carbonyl, carboxyl, etc.), and the strong interaction between the hydroxyl groups on the surface of the activated carbon fiber and the polymethyl methacrylate microspheres enables it to be spontaneously wrapped on the surface of the polymethyl methacrylate microspheres, and then the polymethyl methacrylate microspheres are pyrolyzed in situ to obtain highly conductive three-dimensional porous carbon fibers, which can reduce the material density, introduce more conductive interfaces, and achieve lightweight and high electromagnetic shielding performance. By compounding basalt fiber, three-dimensional porous carbon fiber, modified graphene and epoxy resin, using modified graphene as an electromagnetic shielding functional layer, forming a continuous conductive path in the composite material and using a porous structure to enhance multiple reflections of electromagnetic waves, thereby improving the electromagnetic shielding performance of the material. Using three-dimensional porous carbon fiber as a bridge to connect basalt fiber and modified graphene, a conductive network is constructed in the composite material, forming a larger interface area and more multiple reflection surfaces, so that current accumulation is formed inside, thereby effectively dissipating electromagnetic waves in the form of heat energy, and enhancing the absorption loss of electromagnetic waves by the material.
[0014] In the preparation method, the adhesion of dopamine is utilized to adhere polydopamine to the surface of basalt fiber, and dopamine is used as a bridge to graft nano-silicon dioxide to the surface of basalt fiber through the high content of active functional groups on the surface of polydopamine, thereby enhancing the chemical bonding between the fiber and the resin matrix, and enhancing the impact strength, bending strength and wear resistance of the material. The use of surfactants can improve the dispersion of carbon fiber in deionized water, so that the carbon fiber dispersion has better uniformity, and the carbon fiber can better wrap the polymethyl methacrylate microspheres, forming a more stable three-dimensional structure, thereby improving the electromagnetic shielding performance of the three-dimensional porous carbon fiber. The surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene are laid and stacked in sequence, and epoxy resin is poured to form a laminated composite structure. The conductive network structure introduced in the system strengthens the multiple reflection loss of electromagnetic waves on the inner wall of the material, and the heterogeneous structure formed by the strong interaction between the layers further improves the interface polarization loss capacity, so that the material has excellent electromagnetic shielding performance. DETAILED DESCRIPTION
[0015] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0016] The present embodiment provides a basalt-based shielding material, comprising the following raw materials in parts by weight: 10-20 parts of basalt fiber, 1-10 parts of activated carbon fiber, 5-12 parts of modified graphene, 10-20 parts of epoxy resin, 1-5 parts of polymethyl methacrylate microspheres, 1-5 parts of surfactant and 1-5 parts of curing agent.
[0017] Basalt fiber has excellent tensile properties, strong corrosion resistance and chemical stability, good thermal stability, etc. Basalt fiber is an insulating material, which limits its application in electromagnetic shielding, electrostatic protection and other fields. By compounding basalt fiber, three-dimensional porous carbon fiber, modified graphene and epoxy resin, using modified graphene as the electromagnetic shielding functional layer, forming a continuous conductive path in the composite material and using the porous structure to enhance the multiple reflections of electromagnetic waves, the electromagnetic shielding performance of the material is improved. Using three-dimensional porous carbon fiber as a bridge to connect basalt fiber and modified graphene, a conductive network is constructed in the composite material, forming a larger interface area and more multiple reflection surfaces, so that current accumulation is formed inside, thereby effectively dissipating electromagnetic waves in the form of heat energy, and enhancing the material's absorption loss of electromagnetic waves.
[0018] The surface of activated carbon fiber has more active groups (hydroxyl, carbonyl, carboxyl, etc.). The strong interaction between the hydroxyl groups on the surface of activated carbon fiber and the polymethyl methacrylate microspheres enables it to spontaneously wrap on the surface of polymethyl methacrylate microspheres, and then the polymethyl methacrylate microspheres are pyrolyzed in situ to obtain highly conductive three-dimensional porous carbon fibers, which can reduce the material density, introduce more conductive interfaces, and achieve lightweight and high electromagnetic shielding performance.
[0019] Specifically, the activation method of activated carbon fiber is as follows: heat-treat the carbon fiber in a muffle furnace at 400℃ for 1h, then transfer it to an acetone solution and soak it for 12h to remove the sizing agent on the surface of the carbon fiber; then ultrasonically treat the carbon fiber in deionized water at 60℃ for 30min, then add it to concentrated nitric acid at 60℃ and soak it for 20min and then ultrasonically treat it for 30min. The number of oxygen-containing functional groups on the surface of the carbon fiber after the sizing agent is removed is small. Ultrasonication in deionized water produces free radicals such as -OH in the aqueous solution under the action of ultrasonic cavitation effect, which causes a certain degree of oxidation on the surface of the carbon fiber. Through soaking in concentrated nitric acid, the surface of the carbon fiber is oxidized by concentrated nitric acid to increase the content of oxygen-containing functional groups such as hydroxyl, carbonyl, carboxyl and lactone on the fiber surface, thereby increasing the oxygen content on the surface of the carbon fiber. Then ultrasonic treatment, the cavitation effect of ultrasound further promotes the oxidation and decoration of the carbon fiber surface, and the synergistic effect of the two greatly improves the O / C ratio on the surface of the carbon fiber and increases the surface active groups. In addition, the activation treatment can also increase the roughness of the carbon fiber surface, improve the wettability and reactivity of the carbon fiber with the resin, and enhance the interfacial bonding strength of the composite material.
[0020] Graphene is a single-layer film composed of carbon atoms, only one atom thick, with many unique physical properties, such as extremely high electrical conductivity, thermal conductivity and strength. In addition, graphene also has strong absorption capacity and optical transmittance. Graphene has extremely high electrical conductivity and transparency, and can absorb and exclude electromagnetic waves very well.
[0021] As a polymer material, epoxy resin has good insulation, mechanical strength and corrosion resistance. Epoxy resin can also play a certain role in electromagnetic wave shielding. Specifically, the conductive property of epoxy resin can be achieved by adding carbon fiber or metal filler. The better the conductive property, the better the electromagnetic wave shielding effect.
[0022] Furthermore, the raw materials also include 1-5 parts of nano silicon dioxide by weight. Silicon dioxide is a ceramic material with good electrical conductivity and is often used in the field of electromagnetic wave shielding. Nano silicon dioxide has a small particle size and high surface activity. When introduced into the basalt fiber / resin system, it can increase the surface roughness of the fiber, increase the wettability of the fiber and the resin, promote stress transfer between the fiber and the resin, and thus improve the interfacial adhesion between the carbon fiber and the resin.
[0023] Furthermore, the surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate, ammonium dodecyl sulfate and sodium tetradecyl sulfate.
[0024] Furthermore, the curing agent is one or more of ethylenediamine, triethylenetetramine, maleic anhydride, aniline, titanic anhydride and cyclic phenolic anhydride.
[0025] This embodiment provides a method for preparing a basalt-based shielding material, comprising the following steps:
[0026] S1. Immerse basalt fiber in dopamine solution for polymerization reaction, wash with water, and dry to obtain polydopamine-coated basalt fiber, add nano-silicon dioxide into buffer solution for ultrasonic treatment, then add polydopamine-coated basalt fiber, stir, and dry to obtain surface-modified basalt fiber; utilize the adhesion of dopamine to adhere polydopamine to the surface of basalt fiber, use dopamine as a bridge, and graft nano-silicon dioxide to the surface of basalt fiber through the high content of active functional groups on the surface of polydopamine, so as to enhance the chemical bonding between fiber and resin matrix, and enhance the impact strength, bending strength and wear resistance of the material; at the same time, nano-silicon dioxide and basalt fiber can be grafted to produce conductive basalt fiber.
[0027] S2. Then, an activated carbon fiber dispersion is prepared using a surfactant, and polymethyl methacrylate microspheres are added to the activated carbon fiber dispersion for mixing, freeze-drying, and heat treatment to obtain three-dimensional porous carbon fibers. The surfactant can be used to improve the dispersion of the carbon fiber in deionized water, so that the carbon fiber dispersion has better uniformity, the carbon fiber can better wrap the polymethyl methacrylate microspheres, and the formed three-dimensional structure is more stable, thereby improving the electromagnetic shielding performance of the three-dimensional porous carbon fiber.
[0028] S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature, and then cure at 60-65° C. to obtain the basalt-based shielding material.
[0029] In step S1, the polymerization reaction is carried out at room temperature for 8-12 hours, the buffer is Tris buffer with a concentration of 10 mM / L and a pH of 8.5, and the ultrasonic treatment is carried out for 20-40 minutes.
[0030] In step S1, the nano-silicon dioxide is activated, and the process is as follows: the nano-silicon dioxide and the anhydrous ethanol solution are mixed in a mass ratio of 1:20, ultrasonically treated for 30 minutes, a silane coupling agent is added at 75°C, stirred for 4 hours, centrifuged and washed, and dried at 75°C to obtain activated nano-silicon dioxide. By activating the nano-silicon dioxide, the functional groups on the surface of the nano-silicon dioxide can be increased, so that the grafting rate of the nano-silicon dioxide on the surface of the basalt fiber is higher, so as to significantly improve the mechanical properties of the basalt fiber.
[0031] In step S2, heat treatment is performed at 250-300°C for 1 h in an Ar environment.
[0032] The modification steps of modified graphene are as follows: washing the graphene with anhydrous ethanol and deionized water, and then soaking it in a pyrrole monomer solution for 30-40 minutes; mixing an oxidant and a dopant to obtain a mixed solution, slowly adding the mixed solution to the pyrrole monomer solution in which the graphene is soaked, and performing a polymerization reaction for 5-6 hours, and then washing it with anhydrous ethanol and deionized water, and drying it. Among them, the oxidant is ferric chloride, and the dopant is sodium 5-sulfosalicylate. In-situ polymerization of polypyrrole on the graphene surface can form multiple interfaces such as polypyrrole-polypyrrole, polypyrrole-graphene, and graphene-graphene, resulting in interface polarization, causing multiple dielectric relaxations, and the formation of an external conductive path, thereby obtaining excellent electromagnetic shielding effectiveness.
[0033] Polypyrrole is a conductive polymer composed of conjugated single and double bonds. Depositing polypyrrole on graphene through in-situ polymerization can improve the conductivity of graphene on the one hand, and solve the application difficulty of polypyrrole being insoluble and infusible on the other hand. During the redox reaction of pyrrole, the dopant embeds / removes electrons in the polypyrrole conjugated long molecular chain to form charge carriers, which can move along the polypyrrole long chain and improve the conductivity of polypyrrole.
[0034] Example 1
[0035] A basalt-based shielding material, comprising the following raw materials:
[0036] 15g basalt fiber, 5g activated carbon fiber, 10g modified graphene, 15g epoxy resin, 3g polymethyl methacrylate microspheres, 2g surfactant, 1 curing agent, 3g nano-silicon dioxide; wherein the surfactant is sodium dodecylbenzene sulfonate and the curing agent is triethylenetetramine;
[0037] Preparation of activated carbon fiber:
[0038] The carbon fiber was heat treated in a muffle furnace at 400°C for 1 hour, and then transferred to an acetone solution and soaked for 12 hours to remove the sizing agent on the surface of the carbon fiber; the carbon fiber was then ultrasonically treated in deionized water at 60°C for 30 minutes, and then added to concentrated nitric acid at 60°C and soaked for 20 minutes and then ultrasonically treated for 30 minutes;
[0039] Preparation of modified graphene:
[0040] The graphene was washed with anhydrous ethanol and deionized water, and then immersed in a pyrrole monomer solution for 30 minutes; an oxidant and a dopant were mixed to obtain a mixed solution, and the mixed solution was slowly added to the pyrrole monomer solution in which the graphene was immersed, and a polymerization reaction was carried out for 5 hours, and then washed with anhydrous ethanol and deionized water, and dried;
[0041] Activation of Nano-Silica:
[0042] Nano-silica and anhydrous ethanol solution were mixed in a mass ratio of 1:20, ultrasonically treated for 30 min, silane coupling agent was added at 75°C, stirred for 4 h, centrifuged and washed, and dried at 75°C;
[0043] Preparation of shielding materials:
[0044] S1, immersing basalt fiber in dopamine solution, polymerizing at room temperature for 10 hours, washing with water, and drying to obtain polydopamine-coated basalt fiber, adding nano-silicon dioxide to Tris buffer with a concentration of 10 mM / L and a pH of 8.5, ultrasonically treating for 30 minutes, then adding polydopamine-coated basalt fiber, stirring for 24 hours, and drying at 80°C to obtain surface-modified basalt fiber;
[0045] S2, then using a surfactant to prepare an activated carbon fiber dispersion, adding polymethyl methacrylate microspheres to the activated carbon fiber dispersion, stirring vigorously for 2 hours in an Ar environment, freezing the suspension with liquid nitrogen, freeze-drying, and heat-treating at 280° C. for 1 hour in an Ar environment to obtain a three-dimensional porous carbon fiber;
[0046] S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature for 24 hours, and then cure at 65° C. for 2 hours to obtain the basalt-based shielding material.
[0047] Example 2
[0048] A basalt-based shielding material, comprising the following raw materials:
[0049] 10g basalt fiber, 1g activated carbon fiber, 5g modified graphene, 10g epoxy resin, 1g polymethyl methacrylate microspheres, 1g surfactant, 2g curing agent, 1g nano-silicon dioxide; wherein the surfactant is sodium dodecylbenzene sulfonate and the curing agent is maleic anhydride;
[0050] Preparation of activated carbon fiber:
[0051] The carbon fiber was heat treated in a muffle furnace at 400°C for 1 hour, and then transferred to an acetone solution and soaked for 12 hours to remove the sizing agent on the surface of the carbon fiber; the carbon fiber was then ultrasonically treated in deionized water at 60°C for 30 minutes, and then added to concentrated nitric acid at 60°C and soaked for 20 minutes and then ultrasonically treated for 30 minutes;
[0052] Preparation of modified graphene:
[0053] The graphene was washed with anhydrous ethanol and deionized water, and then immersed in a pyrrole monomer solution for 35 minutes; an oxidant and a dopant were mixed to obtain a mixed solution, and the mixed solution was slowly added to the pyrrole monomer solution in which the graphene was immersed, and a polymerization reaction was carried out for 5.5 hours, and then washed with anhydrous ethanol and deionized water, and dried;
[0054] Activation of Nano-Silica:
[0055] Nano-silica and anhydrous ethanol solution were mixed in a mass ratio of 1:20, ultrasonically treated for 30 min, silane coupling agent was added at 75°C, stirred for 4 h, centrifuged and washed, and dried at 75°C;
[0056] Preparation of shielding materials:
[0057] S1. Immerse the basalt fiber in a dopamine solution, polymerize at room temperature for 8-12 hours, wash with water, and dry to obtain polydopamine-coated basalt fiber. Add nano-silicon dioxide to a Tris buffer solution with a concentration of 10 mM / L and a pH of 8.5, perform ultrasonic treatment for 20 minutes, then add the polydopamine-coated basalt fiber, stir for 24 hours, and dry at 80°C to obtain a surface-modified basalt fiber.
[0058] S2, then using a surfactant to prepare an activated carbon fiber dispersion, adding polymethyl methacrylate microspheres to the activated carbon fiber dispersion and mixing, vigorously stirring for 2 hours in an Ar environment, freezing the suspension with liquid nitrogen, freeze-drying, and heat-treating at 250° C. for 1 hour in an Ar environment to obtain a three-dimensional porous carbon fiber;
[0059] S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature for 24 hours, and then cure at 60° C. for 2 hours to obtain the basalt-based shielding material.
[0060] Example 3
[0061] A basalt-based shielding material, comprising the following raw materials:
[0062] 20g basalt fiber, 10g activated carbon fiber, 12g modified graphene, 20g epoxy resin, 5g polymethyl methacrylate microspheres, 5g surfactant, 5g curing agent, 5g nano-silica; wherein the surfactant is sodium tetradecyl sulfate and the curing agent is cyclic phenolic anhydride;
[0063] Preparation of activated carbon fiber:
[0064] The carbon fiber was heat treated in a muffle furnace at 400°C for 1 hour, and then transferred to an acetone solution and soaked for 12 hours to remove the sizing agent on the surface of the carbon fiber; the carbon fiber was then ultrasonically treated in deionized water at 60°C for 30 minutes, and then added to concentrated nitric acid at 60°C and soaked for 20 minutes and then ultrasonically treated for 30 minutes;
[0065] Preparation of modified graphene:
[0066] The graphene was washed with anhydrous ethanol and deionized water, and then immersed in a pyrrole monomer solution for 40 minutes; an oxidant and a dopant were mixed to obtain a mixed solution, and the mixed solution was slowly added to the pyrrole monomer solution in which the graphene was immersed, and a polymerization reaction was carried out for 6 hours, and then washed with anhydrous ethanol and deionized water, and dried;
[0067] Activation of Nano-Silica:
[0068] Nano-silica and anhydrous ethanol solution were mixed in a mass ratio of 1:20, ultrasonically treated for 30 min, silane coupling agent was added at 75°C, stirred for 4 h, centrifuged and washed, and dried at 75°C;
[0069] Preparation of shielding materials:
[0070] S1, immersing basalt fiber in dopamine solution, polymerizing for 12 hours at room temperature, washing with water, and drying to obtain polydopamine-coated basalt fiber, adding nano-silicon dioxide to Tris buffer with a concentration of 10 mM / L and a pH of 8.5, ultrasonically treating for 40 minutes, then adding polydopamine-coated basalt fiber, stirring for 24 hours, and drying at 80°C to obtain surface-modified basalt fiber;
[0071] S2, then using a surfactant to prepare an activated carbon fiber dispersion, adding polymethyl methacrylate microspheres to the activated carbon fiber dispersion, stirring vigorously for 2 hours in an Ar environment, freezing the suspension with liquid nitrogen, freeze-drying, and heat-treating at 300° C. for 1 hour in an Ar environment to obtain a three-dimensional porous carbon fiber;
[0072] S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature for 24 hours, and then cure at 65° C. for 2 hours to obtain the basalt-based shielding material.
[0073] Comparative Example 1
[0074] The difference between this comparative example and Example 1 is that the basalt fiber is not surface modified.
[0075] Comparative Example 2
[0076] The difference between this comparative example and Example 1 is that the activated carbon fiber is replaced by carbon fiber.
[0077] Comparative Example 3
[0078] The difference between this comparative example and Example 1 is that the modified graphene is replaced by graphene.
[0079] Comparative Example 4
[0080] The difference between this comparative example and Example 1 is that the nano-silicon dioxide is not activated.
[0081] Comparative Example 5
[0082] The difference between this comparative example and Example 1 is that the stacking order is three-dimensional porous carbon fiber, modified graphene and surface-modified basalt fiber.
[0083] Comparative Example 6
[0084] The difference between this comparative example and Example 1 is that the stacking order is modified graphene, surface-modified basalt fiber and three-dimensional porous carbon fiber.
[0085] Test results
[0086] After the shielding materials prepared in the embodiment and the comparative example were made into test specimens of the same specification, the following items were tested, and the results are shown in Table 1.
[0087] Tensile strength (MPa), standard CB / T 1041-2008;
[0088] Flexural strength (MPa), standard CB / T 9341-2008;
[0089] Electromagnetic shielding effectiveness test (dB), standard CB / T 30142-2013.
[0090] Table 1 Performance test
[0091]
[0092]
[0093] According to Table 1, the shielding material prepared in the embodiment has good tensile strength and flexural strength, and has excellent shielding effectiveness. Since the basalt fiber, carbon fiber, graphene and nano-silicon dioxide used in Comparative Examples 1-4 are not treated, the tensile strength, flexural strength and electromagnetic effectiveness of the materials obtained in the comparative examples are lower than those in Example 1. This is because the active sites on the surface of basalt fiber, carbon fiber, graphene and nano-silicon dioxide are reduced, the interfacial bonding strength with the three-dimensional porous fiber and modified graphene is reduced, and the content of adsorbed epoxy resin is reduced. When laying and stacking in Comparative Examples 5-6, the three-dimensional porous carbon fibers are respectively in the outer layer, resulting in the tensile strength, flexural strength and electromagnetic effectiveness of the materials obtained in Comparative Examples 5-6 being lower than those in Example 1. This is because the three-dimensional porous carbon fibers cannot be used as a bridge to connect the surface-modified basalt fibers and modified graphene, and cannot construct a conductive network structure, thereby affecting its electromagnetic shielding effectiveness.
[0094] In summary, the basalt-based shielding material of the present application has good tensile strength and bending strength, and also has efficient electromagnetic shielding performance.
[0095] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A basalt-based shielding material, characterized in that: The invention comprises the following raw materials in parts by weight: 10-20 parts of basalt fiber, 1-10 parts of activated carbon fiber, 5-12 parts of modified graphene, 10-20 parts of epoxy resin, 1-5 parts of polymethyl methacrylate microspheres, 1-5 parts of surfactant and 1-5 parts of curing agent.
2. The basalt-based shielding material according to claim 1, characterized in that: The raw materials also include 1-5 parts of nano silicon dioxide by weight.
3. The basalt-based shielding material according to claim 1, characterized in that: The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate, ammonium dodecyl sulfate and sodium tetradecyl sulfate.
4. The basalt-based shielding material according to claim 1, characterized in that: The curing agent is one or more of ethylenediamine, triethylenetetramine, maleic anhydride, aniline, titanic anhydride and cyclic phenolic anhydride.
5. The method for preparing the basalt-based shielding material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, immersing basalt fiber in dopamine solution for polymerization reaction, washing with water, drying to obtain polydopamine-coated basalt fiber, adding nano-silicon dioxide into buffer solution for ultrasonic treatment, then adding polydopamine-coated basalt fiber, stirring, drying to obtain surface-modified basalt fiber; S2, then using a surfactant to prepare an activated carbon fiber dispersion, adding polymethyl methacrylate microspheres to the activated carbon fiber dispersion, mixing, freeze-drying, and heat-treating to obtain a three-dimensional porous carbon fiber; S3. Lay and stack the surface-modified basalt fiber, three-dimensional porous carbon fiber and modified graphene in sequence, infuse a mixture of epoxy resin and curing agent, first cure at room temperature, and then cure at 60-65° C. to obtain the basalt-based shielding material.
6. The method for preparing the basalt-based shielding material according to claim 5, characterized in that: In step S1, the polymerization reaction is carried out at room temperature for 8-12 hours, the buffer is a Tris buffer with a concentration of 10 mM / L and a pH of 8.5, and the ultrasonic treatment is carried out for 20-40 minutes.
7. The method for preparing the basalt-based shielding material according to claim 5, characterized in that: In step S1, the nano-silica is also activated. The process is as follows: the nano-silica and anhydrous ethanol solution are mixed in a mass ratio of 1:20, ultrasonically treated for 30 minutes, a silane coupling agent is added at 75°C, stirred for 4 hours, centrifuged and washed, and dried at 75°C to obtain activated nano-silica.
8. The method for preparing the basalt-based shielding material according to claim 5, characterized in that: In step S2, heat treatment is performed at 250-300°C for 1 h in an Ar environment.
9. The method for preparing the basalt-based shielding material according to claim 5, characterized in that: The modification steps of the modified graphene are: washing the graphene with anhydrous ethanol and deionized water, and then soaking it in a pyrrole monomer solution for 30-40 minutes; mixing an oxidant and a dopant to obtain a mixed solution, slowly adding the mixed solution to the pyrrole monomer solution in which the graphene is soaked, performing a polymerization reaction for 5-6 hours, and then washing it with anhydrous ethanol and deionized water, and drying it.
Citation Information
Cited By
Basalt fiber reinforced composite material for notebook computer shell
CN119872013A
Preparation method of cashmere blend fiber fabric
CN121047020A
Basalt fiber reinforced material for wind power blade and preparation method of basalt fiber reinforced material
CN121718147A