Waterproof and anti-aging packing belt and preparation method thereof

By using polylactic acid resin, modified regenerated PET fiber, nanosilicon dioxide and tannin in the packaging tape, the problem of photooxidation degradation and contamination of the packaging tape is solved, and efficient anti-ultraviolet stability is achieved and Improved mechanical properties, extend service life and promote material recycling.

CN119019828AInactive Publication Date: 2024-11-26JIESHOU FENGHUA PLASTICS CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411116148.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The service life of existing packaging tapes is shortened during photooxidation and degradation, especially the damage to PET and PP materials by near-ultraviolet rays is severe, and traditional anti-aging agents are highly contaminated. The anti-aging effect of zinc oxide in the preparation of mixed materials is affected by The degree of dispersion has a great impact.

Method used

Polylactic acid resin, modified regenerated PET fibers, nanosilica and tannin acid are used as raw materials, and the modified regenerated PET fibers and nanosilica are uniformly dispersed in the polylactic acid system through tannin acid coating to form a blended material , enhance the viscosity and interface force of the material, use the ultraviolet absorption capacity of tannin acid to reduce photooxidation, and improve the mechanical and heat resistance of the material through heat treatment.

Benefits of technology

It significantly improves the UV stability and mechanical properties of the packaging belt, reduces the brittleness and contamination of the material, extends the service life, and realizes the recycling and environmental protection of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993672060000071
    Figure BDA0004993672060000071
  • Figure BDA0004993672060000081
    Figure BDA0004993672060000081
Patent Text Reader

Abstract

The invention discloses a waterproof and anti-aging packing belt and a preparation method thereof, and belongs to the technical field of chemical engineering, the packing belt is prepared by taking polylactic acid, modified regenerated PET fiber, nano silicon dioxide and tannic acid as raw materials through melt extrusion. A PET material is recycled to prepare fibers, bio-based tannic acid is used for modification treatment, so that the fibers and polylactic acid form a blending system, tannic acid is used as a bridging point, the interfacial acting force is enhanced, the dispersity of nano silicon dioxide is further improved, tannic acid improves the compatibility of the raw materials while enhancing the aging resistance of the packing belt, multiple raw materials are combined and complemented, and the anti-aging performance of the packing belt is improved. The prepared packing belt has the advantages of biodegradability and recycling in the aspect of environment, and is good in mechanical property, waterproof property and aging resistance in practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical industry, and in particular relates to a waterproof and aging-resistant packing tape and a preparation method thereof. Background Art

[0002] The strapping tape (binding tape) for packaging is made of polyethylene, polypropylene resin and cold-rolled steel strip as the main raw materials, and also made of nylon and polyester as raw materials, and is prepared by extrusion, uniaxial stretching and heat treatment. PP strapping tape (also known as polypropylene strapping tape) and PET strapping tape (also known as plastic steel strapping tape) are produced using polypropylene and PET polyester as raw materials respectively, and are suitable for packaging objects of different weights.

[0003] With the rapid development of the express delivery industry, the use of strapping tape has gradually increased. Whether it is PP strapping tape or PET strapping tape, the sharp increase in usage has brought greater resource and environmental pressure. The development of environmentally friendly recycling strapping tape is the general trend. Due to the excellent biodegradability of polylactic acid, it is widely used in biomedicine, food packaging and agriculture. However, PLA has obvious shortcomings in performance, such as slow crystallization rate, low crystallinity, brittleness and poor heat resistance, which makes its use far behind traditional polymer materials.

[0004] During the use of strapping tape, there is a problem of shortening the service life due to photo-oxidative degradation. Among them, near-ultraviolet rays are particularly harmful to PET and PP due to their short wavelength and high energy. Polylactic acid will also undergo oxidative degradation under light irradiation and decompose into small molecular compounds. Anti-aging agents are generally added to the materials, among which amine antioxidants have the most outstanding protective effect and are also the earliest discovered type with the most varieties, but this type of antioxidant is highly polluting.

[0005] A Chinese invention patent with application number CN202110742968.1 discloses a nano-modified PET strapping tape, which uses waste PET particles, polyethylene, glass fiber, reinforcing agent and zinc oxide as raw materials to prepare PET strapping tape with excellent comprehensive performance. The aging resistance of the strapping tape is improved by adding zinc oxide, and the mechanical properties are improved by glass fiber and crystal reinforcing agent. However, the actual anti-aging effect of zinc oxide in the strapping tape prepared by mixing multiple raw materials will be affected by the degree of dispersion. When the dispersion effect is poor, the anti-aging effect will also be correspondingly poor. Summary of the invention

[0006] The purpose of the present invention is to provide a waterproof and aging-resistant strapping tape and a preparation method thereof, so as to achieve the purpose of improving the aging-resistant performance of the strapping tape.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The present invention provides a waterproof and aging-resistant strapping tape, which comprises the following raw materials by weight:

[0009] 70-100 parts of polylactic acid resin; 5-20 parts of modified recycled PET fiber; 0.5-5 parts of nano silicon dioxide; 1-8 parts of tannic acid.

[0010] Furthermore, the following raw materials are included by weight:

[0011] 80-90 parts of polylactic acid resin; 8-15 parts of modified recycled PET fiber; 0.5-3 parts of nano silicon dioxide; 1-5 parts of tannic acid.

[0012] Furthermore, the modified regenerated PET fiber is prepared by the following method:

[0013] (1) Regenerated PET fibers were prepared by melt spinning of PET regenerated particles, and then washed three times with deionized water after ultrasonic cleaning with anhydrous ethanol, and dried at 70°C to obtain dry regenerated PET fibers. Compared with PET regenerated particles, the surface impurities of the fibers were removed by washing with anhydrous ethanol and deionized water, and the surface modification effect was better;

[0014] (2) dissolving tannic acid and sodium chloride in water to obtain a mixed solution, and adding tris(hydroxymethyl)aminomethane to adjust the pH to 8.0;

[0015] (3) The dried regenerated PET fiber is immersed in the mixed solution and oscillated at room temperature for 6-12 hours. After the reaction is completed, it is rinsed with deionized water and dried at 70°C to obtain the modified regenerated PET fiber. The fiber is completely immersed in the solution and the fiber is in a dispersed state as much as possible to achieve complete surface coverage.

[0016] Furthermore, the mass ratio of the tannic acid to sodium chloride is 1:10.

[0017] Furthermore, the total mass proportion of tannic acid and sodium chloride in the mixed solution is 2-5%.

[0018] The present invention also provides a method for preparing a waterproof and aging-resistant strapping tape, comprising the following steps:

[0019] (1) heating and drying the polylactic acid resin for 12-24 hours, adding the mixture to a mixer, adding tannic acid, and heating and premixing for 2-4 hours to obtain a premix;

[0020] (2) adding modified recycled PET fiber and nano-silicon dioxide to the premix under heat preservation conditions, stirring for 1-3 hours, and then extruding through a twin-screw extruder to form a ribbon-shaped preform;

[0021] (3) After the strip-shaped blank is cooled, it is heated, stretched and heat-set to prepare a strapping tape.

[0022] Further, the heating and drying temperature is 60-80°C;

[0023] Furthermore, the heating premixing temperature is 185-195°C.

[0024] Furthermore, the heating and stretching temperature is 80-100°C.

[0025] Furthermore, the heat setting treatment temperature is 125-145° C., and the heat setting time is 5-12 minutes.

[0026] Beneficial effects of the present invention:

[0027] (1) The present invention adopts melt spinning and modification of recycled PET particles to obtain modified recycled PET fibers, and combines them with polylactic acid, nano-silicon dioxide and tannic acid to prepare packaging tape. The selected raw material polylactic acid has excellent biodegradability. The recycled PET particles can reduce costs and realize the recycling of PET materials. Tannic acid comes from natural plants and has little environmental pollution.

[0028] (2) By coating modified recycled PET fibers with tannic acid and blending modified polylactic acid, tannic acid is added to the polylactic acid system as a dendrimer, which has a chain entanglement effect, increases the viscosity of the polylactic acid system, and can hinder the expansion of cracks and improve the fracture strength. When adding modified recycled PET fibers for blending, the tannic acid hydroxyl groups on the fiber surface and the tannic acid hydroxyl groups in the polylactic acid form hydrogen bonds, and the tannic acid acts as a bridge point between the fiber and the resin, increasing the interfacial force. There are a large number of defect sites on the surface of the silica nanoparticles, which can interact with the tannic acid, and the nano-silica is evenly dispersed in the polylactic acid system.

[0029] (3) The large amount of phenolic hydroxyl groups contained in the tannic acid structure can scavenge free radicals and active oxygen. Polyphenols have strong ultraviolet absorption at a wavelength of 270-320nm, and the absorption effect is even stronger in the far ultraviolet region with high energy and greater destructive power. They can reduce the photooxidation effect of ultraviolet light and improve the anti-ultraviolet stability of the material.

[0030] (4) Polylactic acid is selected as the raw material. Since polylactic acid has more ester groups and methyl groups on its surface, it has good water resistance. PET fiber has excellent elasticity and breaking strength. Nano-silicon dioxide can improve mechanical properties and heat resistance. The packaging tape prepared by combining the three has both mechanical properties and waterproof properties. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] Regenerated PET fibers were prepared by melt spinning with PET recycled particles as raw materials, washed three times with deionized water after ultrasonic cleaning with anhydrous ethanol, and dried at 70°C to obtain dry regenerated PET fibers. Tannic acid and sodium chloride were mixed in a mass ratio of 1:10, dissolved in water to obtain a mixed solution with a mass concentration of 2%, tris(hydroxymethyl)aminomethane was added to adjust the pH to 8, and the dried regenerated PET fibers were immersed in the mixed solution, shaken and reacted at room temperature for 6 hours, rinsed with deionized water after the reaction was completed, and dried at 70°C to obtain modified regenerated PET fibers.

[0034] 80 parts of polylactic acid resin were dried at 60°C for 24 hours and then added to a mixer, and 1 part of tannic acid was added and premixed at 185°C for 2 hours to obtain a premix. 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under heat preservation conditions. After stirring for 1 hour, the premix was extruded through a twin-screw extruder to form a strip-shaped blank. After cooling, the premix was heated and stretched at 80°C and heat-set at 125°C for 12 minutes to prepare a strapping tape.

[0035] Example 2

[0036] Different from Example 1, the amount of tannic acid added to the premix is ​​3 parts, and the other steps are the same as Example 1.

[0037] Example 3

[0038] Different from Example 1, the amount of tannic acid added to the premix is ​​5 parts, and the other steps are the same as Example 1.

[0039] Example 4

[0040] Different from Example 1, the amount of modified recycled PET fiber added is 11 parts, and the other steps are the same as Example 1.

[0041] Example 5

[0042] Different from Example 1, the amount of modified recycled PET fiber added is 15 parts, and the other steps are the same as Example 1.

[0043] Example 6

[0044] Different from Example 1, the amount of nano silicon dioxide added is 1.5 parts, and the other steps are the same as Example 1.

[0045] Example 7

[0046] Different from Example 1, the amount of nano silicon dioxide added is 3 parts, and the other steps are the same as Example 1.

[0047] Example 8

[0048] Regenerated PET fibers were prepared by melt spinning with PET recycled particles as raw materials, washed three times with deionized water after ultrasonic cleaning with anhydrous ethanol, and dried at 70°C to obtain dry regenerated PET fibers. Tannic acid and sodium chloride were mixed in a mass ratio of 1:10, added to water to dissolve to obtain a mixed solution with a mass concentration of 3.5%, tris(hydroxymethyl)aminomethane was added to adjust the pH to 8, and the dried regenerated PET fibers were immersed in the mixed solution, shaken and reacted at room temperature for 8 hours, rinsed with deionized water after the reaction was completed, and dried at 70°C to obtain modified regenerated PET fibers.

[0049] 90 parts of polylactic acid resin were dried at 70°C for 18 hours and then added to a mixer, and 1 part of tannic acid was added and premixed at 190°C for 3 hours to obtain a premix. 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under heat preservation conditions. After stirring for 2 hours, the premix was extruded through a twin-screw extruder to form a strip-shaped blank. After cooling, the premix was heated and stretched at 90°C and heat-set at 135°C for 9 minutes to prepare a strapping tape.

[0050] Example 9

[0051] Regenerated PET fibers were prepared by melt spinning with PET recycled particles as raw materials, and washed three times with deionized water after ultrasonic cleaning with anhydrous ethanol, and dried at 70°C to obtain dry regenerated PET fibers. Tannic acid and sodium chloride were mixed in a mass ratio of 1:10, added to water to dissolve to obtain a mixed solution with a mass concentration of 5%, tris(hydroxymethyl)aminomethane was added to adjust the pH to 8, and the dried regenerated PET fibers were immersed in the mixed solution, and oscillated at room temperature for 12 hours. After the reaction was completed, they were rinsed with deionized water and dried at 70°C to obtain modified regenerated PET fibers.

[0052] 100 parts of polylactic acid resin were dried at 80°C for 24 hours and then added to a mixer, and 1 part of tannic acid was added and premixed at 190°C for 3 hours to obtain a premix. 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under heat preservation conditions. After stirring for 3 hours, the premix was extruded through a twin-screw extruder to form a strip-shaped blank. After cooling, the premix was heated and stretched at 100°C and heat-set at 145°C for 5 minutes to prepare a strapping tape.

[0053] Comparative Example 1

[0054] In Comparative Example 1, only polylactic acid was used to prepare the strapping tape.

[0055] 80 parts of polylactic acid resin were dried at 60°C for 24 hours, melted at 195°C and extruded through a twin-screw extruder to form a strip-shaped blank. After cooling, the strip was stretched at 80°C and heat-set at 125°C for 12 minutes to prepare a strapping tape.

[0056] Comparative Example 2

[0057] In Comparative Example 1, the regenerated PET fiber was not subjected to modification treatment, and tannic acid was not added to the premix.

[0058] Regenerated PET fiber was prepared by melt spinning with PET recycled particles as raw materials. 80 parts of polylactic acid resin were dried at 110°C for 24 hours and then added into a mixer. They were premixed at 185°C for 2 hours to obtain a premix. 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under heat preservation conditions. After stirring for 1 hour, the premix was extruded into a strip-shaped blank by a twin-screw extruder. After cooling, the premix was heated and stretched at 80°C and heat-set at 125°C for 12 minutes to prepare a strapping tape.

[0059] Comparative Example 3

[0060] In Comparative Example 1, the regenerated PET fiber was not subjected to modification treatment.

[0061] Regenerated PET fiber was prepared by melt spinning with PET recycled particles as raw materials. 80 parts of polylactic acid resin were dried at 60°C for 24 hours and then added to a mixer. 1 part of tannic acid was added and premixed at 185°C for 2 hours to obtain a premix. 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under insulation conditions. After stirring for 1 hour, the premix was extruded through a twin-screw extruder to form a strip-shaped blank. After cooling, the premix was heated and stretched at 80°C and heat-set at 125°C for 12 minutes to prepare a strapping tape.

[0062] Comparative Example 4

[0063] In Comparative Example 1, tannic acid is not added to the premix.

[0064] Regenerated PET fibers were prepared by melt spinning with PET recycled particles as raw materials, washed three times with deionized water after ultrasonic cleaning with anhydrous ethanol, and dried at 70°C to obtain dry regenerated PET fibers. Tannic acid and sodium chloride were mixed in a mass ratio of 1:10, dissolved in water to obtain a mixed solution with a mass concentration of 2%, tris(hydroxymethyl)aminomethane was added to adjust the pH to 8, and the dried regenerated PET fibers were immersed in the mixed solution, shaken and reacted at room temperature for 6 hours, rinsed with deionized water after the reaction was completed, and dried at 70°C to obtain modified regenerated PET fibers.

[0065] 80 parts of polylactic acid resin were dried at 60°C for 24 hours and then added to a mixer, premixed at 185°C for 2 hours to obtain a premix, 8 parts of modified recycled PET fiber and 0.5 parts of nano-silicon dioxide were added under heat preservation conditions, stirred for 1 hour, and extruded into a strip-shaped blank by a twin-screw extruder, which was heated and stretched at 80°C after cooling, and heat-set at 125°C for 12 minutes to prepare a strapping tape.

[0066] The strapping tapes prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were cut into sizes with a width of 10.0 mm and a thickness of 0.8 mm, and performance tests were performed. The results are shown in Table 1.

[0067] Refer to QB / T 4010-2010 "Polyester Strapping Tape" for minimum tensile breaking load and elongation at break tests.

[0068] Refer to GB / T 16422.3-2014 "Plastics Laboratory Light Source Exposure Test Method Part 3: Fluorescent Ultraviolet Lamp" to test the aging resistance. Set the exposure conditions of the strapping tape according to cycle number 1 in 7.5, and test the retention rate of elongation at break after exposure.

[0069] The contact angle of distilled water on the surface of the strapping tape was measured using a contact angle meter at room temperature.

[0070] With reference to GB T 7141-2008 "Test Method for Thermal Aging of Plastics", a forced ventilation thermal aging test chamber was used, the exposure temperature was set at 60°C, and the time was 60h to detect the retention rate of the elongation at break of the strapping tape.

[0071] Table 1

[0072]

[0073]

[0074] It can be seen from Table 1 that when a small amount of tannic acid is added in Examples 1-3, it is beneficial to enhance the intermolecular force and improve the tensile resistance. When the addition amount reaches 5 parts, the PLA segment cannot be well stretched due to the short molecular chain of tannic acid embedded in the main chain of PLA macromolecules, and its tensile performance is slightly reduced. After the addition of tannic acid, the UV aging resistance is significantly improved.

[0075] In Examples 4 and 5, modified recycled PET fibers were added, and the mechanical properties of the strapping tape were significantly improved. In Examples 6 and 7, the heat resistance was significantly improved with the addition of nano-silicon dioxide. In Examples 8 and 9, too much polylactic acid increased the brittleness of the strapping tape, and the hydrophobic contact angle of the polylactic acid became larger, and the heat aging resistance was better than that of Example 1.

[0076] The mechanical properties of the pure polylactic acid strapping tape prepared in Comparative Example 1 are poor. Compared with Example 1, Comparative Examples 2-4 are not conducive to the mechanical properties of the strapping tape due to the reduced intermolecular binding force, whether the fiber is not modified with tannic acid or tannic acid is not added to the premix. Among them, the lack of tannic acid in the premix has a greater impact on the mechanical properties. In Comparative Example 2, due to the lack of tannic acid modification and the addition of tannic acid in the premix, the retention rate of elongation at break after ultraviolet irradiation of the strapping tape in Example 1 is greatly reduced.

[0077] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A waterproof and aging-resistant strapping tape, characterized in that: The following raw materials are included by weight: 70-100 parts of polylactic acid resin; 5-20 parts of modified recycled PET fiber; 0.5-5 parts of nano silicon dioxide; 1-8 parts of tannic acid.

2. The waterproof and aging-resistant strapping tape according to claim 1, characterized in that: The following raw materials are included by weight: 80-90 parts of polylactic acid resin; 8-15 parts of modified recycled PET fiber; 0.5-3 parts of nano silicon dioxide; 1-5 parts of tannic acid.

3. The waterproof and aging-resistant strapping tape according to claim 1, characterized in that: The modified regenerated PET fiber is prepared by the following method: (1) preparing regenerated PET fibers by melt spinning of PET regenerated pellets, washing with anhydrous ethanol ultrasonically, washing with deionized water three times, and drying at 70° C. to obtain dry regenerated PET fibers; (2) dissolving tannic acid and sodium chloride in water to obtain a mixed solution, and adding tris(hydroxymethyl)aminomethane to adjust the pH to 8.0; (3) The dried regenerated PET fiber is immersed in the mixed solution, and oscillated to react at room temperature for 6-12 hours. After the reaction is completed, it is rinsed with deionized water and dried at 70°C to obtain the modified regenerated PET fiber.

4. The waterproof and aging-resistant strapping tape according to claim 3, characterized in that: The mass ratio of the tannic acid to sodium chloride is 1:

10.

5. The waterproof and aging-resistant strapping tape according to claim 3, characterized in that: The total weight proportion of tannic acid and sodium chloride in the mixed solution is 2-5%.

6. A method for preparing a waterproof and aging-resistant strapping tape according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) heating and drying the polylactic acid resin for 12-24 hours, adding the mixture to a mixer, adding tannic acid, and heating and premixing for 2-4 hours to obtain a premix; (2) adding modified recycled PET fiber and nano-silicon dioxide to the premix under heat preservation conditions, stirring for 1-3 hours, and then extruding through a twin-screw extruder to form a ribbon-shaped preform; (3) After the strip-shaped blank is cooled, it is heated, stretched and heat-set to prepare a strapping tape.

7. The method for preparing a waterproof and aging-resistant strapping tape according to claim 6, characterized in that: The heating and drying temperature is 60-80°C.

8. The method for preparing a waterproof and aging-resistant strapping tape according to claim 6, characterized in that: The heating premixing temperature is 185-195°C.

9. The method for preparing a waterproof and aging-resistant strapping tape according to claim 6, characterized in that: The heating and stretching temperature is 80-100°C.

10. The method for preparing a waterproof and aging-resistant strapping tape according to claim 6, characterized in that: The heat setting treatment temperature is 125-145° C., and the heat setting time is 5-12 minutes.

Citation Information

Cited By

  • Anti-blue-light and anti-ultraviolet polyester film as well as preparation method and application thereof

    CN120620602A

  • A blue light blocking and UV-resistant polyester film, its preparation method and application

    CN120620602B

  • Anti-aging thread gluing material and preparation process thereof

    CN121023675A

  • High-strength anti-aging plastic steel packaging tape

    CN121182154A