Formaldehyde-free impregnating adhesive for decorative paper as well as preparation method and application of formaldehyde-free impregnating adhesive

By using a dextile-free impregnated adhesive composed of polyacrylic acid aqueous solution, the problem of the water resistance, scratch resistance and glue strength of the dextile-free impregnated adhesive is solved, formaldehyde-free release and bubble removal are achieved, and the hardness of the decorative paper is improved and Stain resistance.

CN119019958AInactive Publication Date: 2024-11-26SUZHOU FINESET MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411495540.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the production and use of existing legacy-free impregnated glue, there are problems such as poor water resistance, scratch resistance and surface glue strength not meeting standards. In addition, bubbles are prone to occur during drying, resulting in difficulty in winding and cannot be used in practice.

Method used

Aldehyde-free impregnated adhesive composed of polyacrylic acid aqueous solution, organic polyol, polyvinyl alcohol, filler, mold release agent, hydrophobic agent, water, catalyst, etc., is prepared by processing specific formulas and processes. Decorative paper with high hardness and good wear resistance after integration.

Benefits of technology

The formaldehyde-free impregnated glue is realized, which avoids bubble problems, improves the surface bonding strength and stain resistance, and meets the high hardness, wear and stain resistance requirements of decorative paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of decorative paper processing, and discloses a formaldehyde-free impregnating adhesive for decorative paper, which is prepared from the following raw materials in parts by weight: 80 to 100 parts of polyacrylic acid aqueous solution, 5 to 10 parts of organic polyol, 2 to 6 parts of polyvinyl alcohol, 10 to 20 parts of filler, 2 to 5 parts of release agent, 2 to 5 parts of water repellent agent, 30 to 40 parts of water and 0.5 to 2 parts of catalyst. The molecular weight of the polyacrylic acid aqueous solution is 5000-20000, the solid content is 30-50%, and the pH value of the solution is 3-5; the molecular weight of the polyvinyl alcohol ranges from 10000 to 30000, and the viscosity of the polyvinyl alcohol ranges from 4 cps to 6 cps. No formaldehyde is generated in the production and use processes of the impregnating adhesive, the impregnating adhesive is environment-friendly, the surface of formaldehyde-free impregnating adhesive veneer paper prepared from the impregnating adhesive is free of bubbles, and a veneer paper artificial board prepared after hot-pressing lamination has excellent hardness, strength, wear resistance and stain resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of decorative paper processing, and in particular to an aldehyde-free impregnating adhesive for decorative paper, a preparation method and application thereof. Background Art

[0002] Impregnated paper is an important material for veneer man-made panels. It can protect and beautify man-made veneer panels because of its high hardness, wear resistance, scratch resistance, high gloss and other excellent properties. It is a kind of special decorative paper coated with resin (i.e. impregnated glue) on both sides by impregnation, and then dried at high temperature to obtain applicable decorative paper (referred to as impregnated paper). The impregnated glue on the surface of the decorative paper mainly plays a protective and beautifying role after curing. It needs to meet the characteristics of high hardness, wear resistance, scratch resistance, high gloss, and stain resistance. The impregnated glue on the back side mainly plays the role of bonding the wood board to ensure that it has sufficient strength to bond with the bare board to prevent falling off and delamination. The production process of impregnated paper requires two impregnations, two drying and cooling processes, and finally it is packaged by cutting or rolling for use. When used, it needs to be hot-pressed to complete the bonding with the bare board and the formation of the embossed pattern on the surface. At present, most decorative papers are made of melamine-formaldehyde as the adhesive on the front and back sides. Although the decorative paper made of melamine-formaldehyde impregnated adhesive has high hardness, friction resistance and high strength, free formaldehyde is released during the production, processing and use, which is harmful to human health. With the improvement of people's requirements for quality of life and environment, the demand for formaldehyde-free impregnated adhesive film paper is becoming more and more urgent.

[0003] The current formaldehyde-free impregnated adhesives mainly include some natural adhesives, such as minerals, animal glues and plant glues, as well as modified bio-based adhesives and polymer formaldehyde-free impregnated adhesives (such as acrylates, polyurethanes, epoxy resins, etc.). At present, these formaldehyde-free impregnated adhesives are not very perfect, and each has some problems. For example, the patent technical document CN109575875A discloses a biomass formaldehyde-free adhesive and its application in the preparation of formaldehyde-free fragrance-releasing fiberboard. Although the adhesive does not release formaldehyde, the weather resistance and water resistance of the bio-based adhesive are poor; for example, the patent technical document CN110450239A discloses a preparation method of a new type of polyurethane formaldehyde-free impregnated adhesive film paper. The adhesive also achieves formaldehyde-free release, but the polyurethane resin adhesive has a large molecular weight, high viscosity, and high cross-linking degree, resulting in poor permeability, so the scratch resistance and surface bonding strength of the impregnated adhesive film paper are insufficient.

[0004] At present, formaldehyde-free impregnated adhesives have problems such as poor water resistance, scratch resistance, and substandard surface bonding strength. In the production and drying process, bubbles are easily formed on both sides of the film paper, making it difficult to roll up and unable to be used in practice. In view of the above problems, the development of a formaldehyde-free impregnated adhesive that is easy to roll up, has high hardness after hot pressing, good wear resistance, and good stain resistance is the research direction that technicians in this field are committed to. Summary of the invention

[0005] The object of the present invention is to overcome the deficiencies of the prior art and provide an aldehyde-free impregnated adhesive for decorative paper.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a formaldehyde-free impregnating adhesive for decorative paper, wherein the raw materials of the adhesive include, by weight: 80-100 parts of polyacrylic acid aqueous solution, 5-10 parts of organic polyol, 2-6 parts of polyvinyl alcohol, 10-20 parts of filler, 2-5 parts of release agent, 2-5 parts of hydrophobic agent, 30-40 parts of water, and 0.5-2 parts of catalyst, wherein the molecular weight of the polyacrylic acid aqueous solution is between 5000-20000, the solid content is between 30-50%, and the pH value of the solution is between 3-5; the molecular weight of the polyvinyl alcohol is between 10000-30000, the viscosity is 4-6cps, and the mass fraction is 10% aqueous solution.

[0007] As a specific implementation, the raw materials of the polyacrylic acid aqueous solution are composed of the following components in parts by weight: 80-100 parts of acrylic acid, 0-15 parts of chain transfer agent, 100-150 parts of deionized water, 1-5 parts of initiator and 1-5 parts of pH adjuster. The preparation method of the polyacrylic acid aqueous solution is as follows: Add 50% deionized water, all the chain transfer agent and 50% initiator into the reactor, then heat it to 75-80°C, and then slowly drop the remaining deionized water, initiator and acrylic acid. After all the raw materials have been added, keep the reaction at 75-80°C for 2-3 hours. Adjust the pH of the product to between 3-5 with a pH adjuster.

[0008] As a specific implementation, the chain transfer agent is a combination of one or more of isopropyl alcohol, sodium bisulfite, mercaptoethanol, mercaptopropanol, mercaptopropionic acid, thioglycolic acid, sodium hypophosphite, and sodium formate. Preferably, the chain transfer agent is isopropyl alcohol.

[0009] Preferably, the raw materials of the polyacrylic acid aqueous solution are composed of the following components in parts by weight: 100 parts of acrylic acid, 10 parts of chain transfer agent, 150 parts of deionized water, 2 parts of initiator and 2 parts of pH adjuster.

[0010] As a specific embodiment, the initiator is one or more of ammonium persulfate, potassium persulfate, sodium persulfate, azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, and azobisisopropylimidazoline. Preferably, the initiator is ammonium persulfate. The pH regulator is sodium hydroxide, potassium hydroxide, calcium hydroxide or sodium carbonate, preferably sodium hydroxide.

[0011] As a specific implementation, the organic polyol is selected from one or more combinations of ethylene glycol, propylene glycol, glycerol, glycolamine, triethanolamine, and pentaerythritol, preferably triethanolamine.

[0012] As a specific implementation manner, the polyvinyl alcohol adopts a polyvinyl alcohol aqueous solution with a molecular weight of 13,000, a viscosity of 46 cps, and a mass fraction of 10%.

[0013] As a specific implementation manner, the filler is one or a combination of nano silicon dioxide, nano titanium dioxide, mica powder, talcum powder, aluminum oxide, and calcium carbonate; the release agent is Lerogu 8161 or Lerogu INT8.

[0014] The filler is preferably a nano-silica sol with a solid content of 20%; the release agent is preferably Lerogu 8161.

[0015] As a specific implementation, the hydrophobic agent is an organosilicon compound or a wax emulsion; the catalyst is a combination of one or more of concentrated sulfuric acid, phosphoric acid, p-toluenesulfonic acid, and dibutyltin oxide.

[0016] The hydrophobic agent is preferably hydrophobic agent 1402 produced by Guangzhou Huitu Material Co., Ltd.; the catalyst is preferably p-toluenesulfonic acid.

[0017] Another object of the present invention is to provide a method for preparing the above-mentioned formaldehyde-free impregnating adhesive for decorative paper, the specific steps of which are as follows: adding all raw materials into a container according to the weight parts of the formula, stirring with a stirrer for 10-20 minutes, and controlling the stirring speed between 500-2000r / min.

[0018] The third object of the present invention is to provide an application of the above-mentioned formaldehyde-free impregnated adhesive for decorative paper, which is used for a formaldehyde-free impregnated adhesive facing paper. The preparation process of the formaldehyde-free impregnated adhesive facing paper is as follows: the formaldehyde-free impregnated adhesive is coated on the facing paper by using an applicator, and the coating thickness is 100-300 μm, and then the coated facing paper is placed in a blast oven at 70-150° C. and baked for 1-5 minutes. Preferably, the temperature is controlled at 85-120° C. and the baking time is 1-3 minutes.

[0019] The fourth object of the present invention is to provide a decorative paper artificial board, which adopts the above-mentioned formaldehyde-free impregnated adhesive facing paper, and the preparation process of the decorative paper artificial board is as follows: the facing paper is laminated on the medium-density fiberboard or particleboard, and hot-pressed by a hot press, the hot-pressing temperature is controlled between 130-230°C, the hot-pressing time is controlled between 30-150s, and the hot-pressing pressure is controlled between 2MPa-15MPa. Preferably, the hot-pressing temperature is controlled between 160-200°C, the hot-pressing time is controlled between 40-90s, and the hot-pressing pressure is controlled between 5-10MPa.

[0020] Due to the application of the above technical scheme, the present invention has the following advantages compared with the prior art: the impregnating adhesive of the present invention adopts polyacrylic acid aqueous solution as the main component, and its solvent is also water. The impregnating adhesive does not produce formaldehyde during the production and use process, and has less harm to the environment and human body. The formaldehyde-free impregnated adhesive facing paper prepared by using the impregnating adhesive has no bubbles on the surface and can be easily rolled up. The facing paper artificial board prepared after hot pressing and bonding has excellent hardness, strength, wear resistance and stain resistance. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0022] Provided below is a formaldehyde-free impregnating adhesive for decorative paper, the raw materials of the adhesive comprising polyacrylic acid aqueous solution, organic polyol, polyvinyl alcohol, filler, release agent, hydrophobic agent, water, and catalyst.

[0023] The molecular weight of the polyacrylic acid aqueous solution here is between 5000-20000, the solid content is between 30-50%, and the pH value of the solution is between 3-5; the molecular weight of the polyvinyl alcohol is between 10000-30000, the viscosity is 4-6cps, and the mass fraction is 10% aqueous solution.

[0024] The organic polyol is selected from one or more combinations of ethylene glycol, propylene glycol, glycerol, glycolamine, triethanolamine, and pentaerythritol, and triethanolamine is preferred.

[0025] The polyvinyl alcohol used was a polyvinyl alcohol aqueous solution with a molecular weight of 13,000, a viscosity of 46 cps, and a mass fraction of 10%.

[0026] The filler is one or a combination of nano silicon dioxide, nano titanium dioxide, mica powder, talcum powder, aluminum oxide, and calcium carbonate, and preferably nano silicon dioxide sol with a solid content of 20% is used.

[0027] The mold release agent is Lerogu 8161 or Lerogu INT8, and Lerogu 8161 is preferably used.

[0028] The hydrophobic agent uses an organosilicon compound or a wax emulsion, and preferably uses the hydrophobic agent 1402 produced by Guangzhou Huitu Materials Co., Ltd.

[0029] The catalyst is a combination of one or more of concentrated sulfuric acid, phosphoric acid, p-toluenesulfonic acid and dibutyltin oxide, and p-toluenesulfonic acid is preferred.

[0030] The polyacrylic acid aqueous solution used in the following examples is composed of the following components in parts by weight: 100 parts of acrylic acid, 10 parts of chain transfer agent isopropanol, 150 parts of deionized water, 2 parts of initiator ammonium persulfate and 2 parts of pH adjuster NaOH. The preparation method of the polyacrylic acid aqueous solution is as follows: Add 50% deionized water, all isopropanol and 50% ammonium persulfate into the reactor, then heat to 75°C, slowly add the remaining deionized water, initiator and acrylic acid, and after all the raw materials have been added, react at 75°C for 2-3 hours. Adjust the pH of the product to between 3-5 with 20% NaOH.

[0031] Acrylic acid: CAS: 79-10-7. Example 1

[0032] In this example, a decorative paper artificial board is provided, and the preparation method thereof is as follows: 1) Preparation of impregnation glue: Add 100 parts of polyacrylic acid aqueous solution, 10 parts of triethanolamine, 5 parts of release agent Lerogu 8161, 5 parts of hydrophobic agent 1402, 6 parts of polyvinyl alcohol, 1.1 parts of p-toluenesulfonic acid, 20 parts of nano-silica solution HA2005, and 40 parts of water into a container, and then stir evenly with a stirrer at a stirring rate of 500r / min~2000r / min; 2) Use an applicator to apply the glue on the decorative paper with a coating thickness of 300 μm, put it into an oven, bake it at 85°C for 3 minutes, stick it on the wooden board after drying, and put it into a hot press for hot pressing at 200°C, 5MPa, and 60s. Example 2

[0033] In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 80 parts of polyacrylic acid aqueous solution, 5 parts of triethanolamine, 2 parts of release agent Lerogu 8161, 2 parts of hydrophobic agent 1402, 2 parts of polyvinyl alcohol, 0.85 parts of p-toluenesulfonic acid, 10 parts of nano-silica solution HA2005, and 30 parts of water. Example 3

[0034] In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 90 parts of polyacrylic acid aqueous solution, 7.5 parts of triethanolamine, 3 parts of release agent Lerogu 8161, 4 parts of hydrophobic agent 1402, 4 parts of polyvinyl alcohol, 0.98 parts of p-toluenesulfonic acid, 15 parts of nano-silica solution HA2005, and 35 parts of water. Example 4

[0035] In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 100 parts of polyacrylic acid aqueous solution, 8 parts of triethanolamine, 4 parts of release agent Lerogu 8161, 3 parts of hydrophobic agent 1402, 3 parts of polyvinyl alcohol, 1.08 parts of p-toluenesulfonic acid, 20 parts of nano-silica solution HA2005, and 40 parts of water. Example 5

[0036] In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 80 parts of polyacrylic acid aqueous solution, 5 parts of triethanolamine, 2 parts of release agent Lerogu 8161, 2 parts of hydrophobic agent 1402, 2 parts of polyvinyl alcohol, 0.9 parts of p-toluenesulfonic acid, 15 parts of nano-silica solution HA2005, and 30 parts of water. Example 6

[0037] In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 90 parts of polyacrylic acid aqueous solution, 6 parts of triethanolamine, 3 parts of release agent Lerogu 8161, 3 parts of hydrophobic agent 1402, 3 parts of polyvinyl alcohol, 0.69 parts of p-toluenesulfonic acid, 12 parts of nano-silica solution HA2005, and 38 parts of water.

[0038] Comparative Example 1 In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 100 parts of polyacrylic acid aqueous solution, 4 parts of triethanolamine, 5 parts of release agent Lerogu 8161, 5 parts of hydrophobic agent 1402, 6 parts of polyvinyl alcohol, 1.1 parts of p-toluenesulfonic acid, 20 parts of nano-silica solution HA2005, and 40 parts of water.

[0039] Comparative Example 2 In this example, a decorative paper artificial board is provided, and its preparation method is the same as that of Example 2, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 80 parts of polyacrylic acid aqueous solution, 5 parts of triethanolamine, 2 parts of release agent Lerogu 8161, 2 parts of polyvinyl alcohol, 0.85 parts of p-toluenesulfonic acid, 10 parts of nano-silica solution HA2005, and 30 parts of water.

[0040] Comparative Example 3 In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 3, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 90 parts of polyacrylic acid aqueous solution, 7.5 parts of triethanolamine, 4 parts of hydrophobic agent 1402, 4 parts of polyvinyl alcohol, 0.98 parts of p-toluenesulfonic acid, 15 parts of nano-silica solution HA2005, and 35 parts of water.

[0041] Comparative Example 4 In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 100 parts of polyacrylic acid aqueous solution, 10 parts of triethanolamine, 5 parts of release agent Lerogu 8161, 5 parts of hydrophobic agent 1402, 6 parts of polyvinyl alcohol, 1.1 parts of p-toluenesulfonic acid, and 40 parts of water.

[0042] Comparative Example 5 In this example, a decorative paper artificial board is provided, and its preparation method is the same as that in Example 1, except that the content of the raw material components of the impregnating glue is different. Specifically, the raw material components of the impregnating glue in this example are as follows: 100 parts of polyacrylic acid aqueous solution, 11 parts of triethanolamine, 5 parts of release agent Lerogu 8161, 5 parts of hydrophobic agent 1402, 6 parts of polyvinyl alcohol, 1.1 parts of p-toluenesulfonic acid, 20 parts of nano-silica solution HA2005, and 40 parts of water.

[0043] Comparative Example 6 This example provides a decorative paper artificial board, whose raw material components and preparation method are the same as those in Example 1, except that the pH of the polyacrylic acid aqueous solution in the raw material components of the impregnated glue is different. The pH of the polyacrylic acid aqueous solution in this example is 1.5.

[0044] Comparative Example 7 This example provides a decorative paper artificial board, whose raw material components and preparation method are the same as those in Example 1, except that the pH of the polyacrylic acid aqueous solution in the raw material components of the impregnated glue is different. The pH of the polyacrylic acid aqueous solution in this example is 7.0.

[0045] The raw material components of the impregnated glue of the decorative paper artificial boards prepared in Examples 1-6 and Comparative Examples 1-7 are shown in Table 1. Performance tests were carried out in accordance with GB / T31905-2015, GB / T28995-2012, GB / T15102-2017 and GB / T17657-2013 standards. The test results are shown in Table 2.

[0046] Table 1

[0047] Among them, PAA is polyacrylic acid aqueous solution; TEA is triethanolamine; PVA is polyvinyl alcohol.

[0048] Table 2

[0049] Note: O means demoulding is possible, and × means demoulding is not possible.

[0050] From Table 2, the difference between Comparative Example 3 and Example 3 lies in the use of a release agent, so it can be seen that if a release agent is not added, demoulding is impossible, and the surface bonding strength and other properties cannot be tested; from Comparative Example 1 compared with Example 1, the amount of triethanolamine added is less than the specified range, the humidity surface stain resistance is poor, and the surface scratch resistance is unqualified; Comparative Example 2 compared with Example 2, no hydrophobic agent is added, resulting in poor surface stain resistance; Comparative Example 4 compared with Example 1, no filler is added, resulting in unqualified surface scratch resistance. Comparative Example 5 compared with Example 1, the amount of triethanolamine added is greater than the specified range, resulting in poor surface stain resistance, because excessive triethanolamine cannot fully participate in the cross-linking reaction, triethanolamine is a surfactant, so it will cause the surface stain resistance to deteriorate. Comparative Example 6 compared with Example 1, the pH value of PAA is less than 3, and the surface stain resistance will deteriorate. Comparative Example 7 compared with Example 1, the pH value of PAA is greater than 5, and the surface stain resistance and scratch resistance will deteriorate.

[0051] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A formaldehyde-free impregnating adhesive for decorative paper, characterized in that: The raw materials of the adhesive include, by weight, 80-100 parts of a polyacrylic acid aqueous solution, 5-10 parts of an organic polyol, 2-6 parts of polyvinyl alcohol, 10-20 parts of a filler, 2-5 parts of a release agent, 2-5 parts of a hydrophobic agent, 30-40 parts of water, and 0.5-2 parts of a catalyst. The polyacrylic acid aqueous solution has a molecular weight of 5,000-20,000, a solid content of 30-50%, and a pH value of 3-5. The polyvinyl alcohol has a molecular weight of 10,000-30,000, a viscosity of 4-6 cps, and a mass fraction of 10% in aqueous solution.

2. The formaldehyde-free impregnating adhesive for decorative paper according to claim 1, characterized in that: The raw materials of the polyacrylic acid aqueous solution are composed of the following components in parts by weight: Composition: 80-100 parts of acrylic acid, 0-15 parts of chain transfer agent, 100-150 parts of deionized water, 1-5 parts of initiator and 1-5 parts of pH adjuster. The preparation method of the polyacrylic acid aqueous solution is as follows: Add 50% deionized water, all the chain transfer agent and 50% initiator to the reactor, then heat it to 75-80°C, and slowly add the remaining deionized water, initiator and acrylic acid. After all the raw materials are added, keep the reaction at a constant temperature of 75-80°C for 2-3 hours. Adjust the pH of the product to between 3-5 with a pH regulator.

3. The formaldehyde-free impregnated adhesive for decorative paper according to claim 2, characterized in that: The chain transfer agent is a combination of one or more of isopropyl alcohol, sodium bisulfite, mercaptoethanol, mercaptopropanol, mercaptopropionic acid, thioglycolic acid, sodium hypophosphite, and sodium formate.

4. The formaldehyde-free impregnated adhesive for decorative paper according to claim 2, characterized in that: The initiator is one or a combination of ammonium persulfate, potassium persulfate, sodium persulfate, azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, and azobisisopropylimidazoline.

5. The formaldehyde-free impregnating adhesive for decorative paper according to claim 1, characterized in that: The organic polyol is selected from one or more combinations of ethylene glycol, propylene glycol, glycerol, glycolamine, triethanolamine, and pentaerythritol.

6. The formaldehyde-free impregnating adhesive for decorative paper according to claim 1, characterized in that: The polyvinyl alcohol used was a polyvinyl alcohol aqueous solution with a molecular weight of 13,000, a viscosity of 46 cps, and a mass fraction of 10%.

7. The formaldehyde-free impregnating adhesive for decorative paper according to claim 1, characterized in that: The filler is one or more of nano-silicon dioxide, nano-titanium dioxide, mica powder, talc, aluminum oxide, and calcium carbonate; the release agent is Lerogu 8161 or Lerogu INT8; the hydrophobic agent is an organosilicon compound or a wax emulsion; and the catalyst is one or more of concentrated sulfuric acid, phosphoric acid, p-toluenesulfonic acid, and dibutyltin oxide.

8. A method for preparing the formaldehyde-free impregnated adhesive for decorative paper according to any one of claims 1 to 7, characterized in that: The specific steps are as follows: add all the raw materials according to the weight of the formula into the container, stir with a stirrer for 10-20 minutes, and control the stirring speed between 500-2000r / min.

9. Use of the formaldehyde-free impregnated adhesive for decorative paper according to any one of claims 1 to 7 for a formaldehyde-free impregnated adhesive facing paper, characterized in that: The preparation process of the formaldehyde-free impregnated adhesive facing paper is as follows: the formaldehyde-free impregnated adhesive is coated on the facing paper using a coater with a coating thickness of 100-300 μm, and then the coated facing paper is placed in a blast oven at 70-150° C. and baked for 1-5 minutes.

10. A decorative paper artificial board, characterized in that: The formaldehyde-free impregnated adhesive facing paper as described in claim 9 is used, and the preparation process of the decorative paper artificial board is as follows: the facing paper is laminated on the medium-density fiberboard or particleboard, and hot-pressed using a hot press, the hot-pressing temperature is controlled between 130-230°C, the hot-pressing time is controlled between 30-150s, and the hot-pressing pressure is between 2MPa-15MPa.

Citation Information

Patent Citations

  • Impregnated adhesive film paper facing aldehyde-free artificial board and preparation method thereof

    CN111496948A

  • Formaldehyde-free impregnated adhesive for decorative paper and preparation method of formaldehyde-free impregnated adhesive

    CN111501416A

  • Hydrophobic dirt-resistant decorative paper and production method thereof

    CN116289332A

  • Dirt-resistant decorative paper and preparation method thereof

    CN118360822A