Method for preparing 5N-grade high-purity metallic antimony

Through the ball milling and pressing process of glucose and antimony white, high-temperature carbonization reduction is carried out in a vacuum furnace, and a one-step distillation is achieved to prepare 5N grade high-purity metal antimony, which solves the problems of low purity of antimony metal and complex process in the existing technology, and realizes the Efficient and safe industrial production.

CN119020612APending Publication Date: 2024-11-26YINTAI SCI & TECH HIGH TECH ZONE LIUZHOU CITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411049654.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, antimony metal has low purity, high refining cost, and complex process, which cannot meet the application needs of high-end fields, especially high-purity hydrogen reduction methods, which pose safety risks.

Method used

After ball milling and refining with glucose and antimony white, the holes are pressed into a hole block and carbonized and reduced in a vacuum furnace at high temperature. One-step distillation is used to obtain 5N high-purity metal antimony, which simplifies the process flow and improves the reduction efficiency and reduces safety risks.

Benefits of technology

It realizes an efficient, safe and simplified 5N high-purity metal antimony preparation process, which is suitable for industrial production, improves the reduction efficiency of antimony white, and reduces process complexity and safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020612A_ABST
    Figure CN119020612A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing 5N-grade high-purity metallic antimony, which is an efficient method suitable for industrial production of 5N high-purity antimony. According to the method, antimony white and glucose are adopted as raw materials, and mixing and refining of antimony white (Sb2O3) and glucose are achieved through the ball milling process. The method comprises the following steps: preparing 5N-grade antimony white (Sb2O3) from 5N-grade antimony white (Sb2O3), then preparing a block body rich in 5-10mm holes through resonance sound mixing and pressing, then carrying out high-temperature carbonization reduction in a vacuum furnace so as to reduce the 5N-grade antimony white (Sb2O3) into metal antimony, and carrying out vacuum distillation to obtain 5N-grade high-purity metal antimony (Sb). The process provided by the invention has the advantage that the preparation process is safer, more efficient and simpler. Carbon reduction which is safer than hydrogen reduction is used, the reduction efficiency of antimony white can be greatly improved through the ball milling technology, the briquetting technology and the integrated distillation technology, the process is simple, and industrial popularization is easy to achieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-purity metal preparation, and relates to a method for preparing 5N-grade high-purity metal antimony. Background Art

[0002] Pure metallic antimony is an important raw material for the preparation of semiconductor components, electronic components, and optoelectronic materials. However, due to the technical and production cost limitations of the domestic metallurgical industry, the purity of the antimony currently extracted is relatively low and cannot meet the application needs of high-end fields such as semiconductors.

[0003] The content of antimony in the earth's crust is 0.0001%, mainly in the form of simple substance or stibnite, stibnite and antimony ochre. At present, the main method of industrial production of metallic antimony is to use a reflective reduction furnace to reduce antimony white to obtain industrial-grade metallic antimony. This method has the advantage of low refining cost, but it also has disadvantages such as low purity of refined antimony metal and insufficient reduction of raw materials leading to waste.

[0004] Therefore, the development of environmentally friendly, efficient and low-cost 5N high-purity antimony metal extraction process is the trend of industry development. Currently, the industry has developed technologies such as distillation or high-purity hydrogen reduction to obtain high-purity antimony metal (Sb). For example:

[0005] The invention with patent number ZL202310734553.9 adopts high temperature pyrolysis to reduce antimony white (Sb 2 O 3 ) is used as antimony, and white sugar is mixed with 5N grade antimony white (Sb 2 O 3 ) and use the carbon generated by carbonization of sugar at high temperature to convert high purity antimony white (Sb 2 O 3 ) into metallic antimony (Sb), and then distilled to obtain 5N grade high-purity metallic antimony (Sb), achieving the effect of highly purified antimony metal. However, this method has the problem of antimony white (Sb 2 O 3 ) and poor utilization of white sugar, and requires step-by-step distillation, which is a complicated process.

[0006] The invention with patent number ZL202310040343 successfully reduces antimony trichloride with high purity by using high purity hydrogen in an atmosphere furnace to reduce high purity metallic antimony (Sb). However, this method uses high purity hydrogen, which is extremely dangerous and requires a very strict production environment.

[0007] In view of the problems existing in the current prior art, the present invention provides a simple, efficient and industrially applicable method for producing high-purity antimony. The method uses ball milling to effectively mix antimony white with glucose and reduce the particle size, and then uses glucose carbon to reduce antimony white (Sb 2 O 3) into metallic antimony (Sb), and then distill it in one step to obtain high-purity metallic antimony (Sb). This technology can effectively improve the reduction efficiency of antimony white and greatly simplify the process flow during the reduction process, and has a higher safety factor than hydrogen reduction. It is suitable for large-scale production of high-purity antimony (Sb) in industry. Summary of the invention

[0008] Technical issues to be solved

[0009] In order to avoid the shortcomings of the prior art, the present invention proposes a method for preparing 5N grade high purity metallic antimony. In view of the problems existing in the current prior art, the present invention provides a simple, efficient and industrially applicable method for producing high purity antimony.

[0010] Technical Solution

[0011] A method for preparing 5N grade high purity antimony metal, characterized by the following steps:

[0012] Step 1: Fully refine and mix glucose and antimony white to form antimony white polysaccharide mixed powder;

[0013] Step 2: pressing the antimony white polysaccharide mixed powder into a porous block;

[0014] Step 3: Place the porous block in a vacuum furnace and heat it at 300℃~1000℃ to perform high temperature carbonization reduction to convert 5N grade antimony white Sb 2 O 3 Reduced to 5N grade metallic antimony.

[0015] The glucose and antimony white are fully refined and mixed by ball milling in a liquid nitrogen environment.

[0016] In step 2, the mixed powder is added into a mold and pressed to obtain a block with distributed holes; the mold has holes with a diameter of 5 to 30 mm, and the holes distributed in the block have a diameter of 5 to 30 mm.

[0017] The ball mill speed during the ball milling is 200r / min to 500r / min.

[0018] During the ball milling, the liquid nitrogen needs to cover the material, and the liquid nitrogen needs to be continuously replenished during the ball milling process.

[0019] The mass ratio of the 5N grade high-purity antimony white to the glucose is 100:15-35.

[0020] The polysaccharide is preferably glucose.

[0021] The heating for high-temperature carbonization reduction in step 3 adopts two heating sections, the first section is kept at room temperature to 300° C. for 2 hours, and then continues to heat up to 500-1000° C. for high-temperature carbonization.

[0022] The heating rate of the first stage adopts two-stage heating, starting from room temperature to 300°C for 2h, and then continuing to heat up to 400-500°C for condensation.

[0023] The vacuum degree of the vacuum furnace is 1x10 -4 Pa~5x10 -2 Pa.

[0024] Beneficial Effects

[0025] The method for preparing 5N grade high-purity metallic antimony proposed in the present invention is an efficient method suitable for industrial production of 5N high-purity antimony. The method uses antimony white and glucose as raw materials, and achieves antimony white (Sb 2 O 3 ) and glucose are mixed and refined. Then, through resonant acoustic mixing and pressing, it is made into a block with 5-10mm pores, and then high-temperature carbonization reduction is carried out in a vacuum furnace to convert 5N grade antimony white (Sb 2 O 3 ) is reduced to metallic antimony and vacuum distilled to obtain 5N grade high-purity metallic antimony (Sb). The process provided by the present invention has the advantages of being safer, more efficient and simpler in preparation. The present invention uses carbon reduction, which is safer than hydrogen reduction, and through ball milling process, briquetting process and integrated distillation process, not only the reduction efficiency of antimony white can be greatly improved, but also the process is simple and easy to realize industrialization and popularization. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 :Schematic diagram of vacuum furnace

[0027] 1- condensation plate, 2- upper heating temperature section (referred to as the upper section), 3- lower heating temperature section (referred to as the lower section) DETAILED DESCRIPTION

[0028] The present invention will now be further described with reference to the embodiments and the accompanying drawings:

[0029] The preparation method is characterized in that: a vacuum furnace is used as a smelting device to melt the 5N grade high purity antimony white (Sb 2 O 3 ) and the glucose in a mass ratio of 100:15-35 and then ball-milled for 10-24 hours. The ball-milled material is pressed into a block with 5-10 mm holes. The block is placed in a vacuum furnace and heated to 300°C at the lower and upper sections for 3 hours, and then the lower end is heated to 500-1000°C to remove antimony white (Sb 2 O 3 ) is reduced to metallic antimony (Sb), and the upper section is heated to 400-500°C to condense the antimony metal. 5N grade high-purity metallic antimony (Sb) is obtained in the upper condensation tray.

[0030] The metallic antimony (Sb) obtained by reducing glucose with antimony white is then further vacuum distilled in a furnace to obtain 5N grade high-purity metal (Sb).

[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below so that those skilled in the art can implement them according to the description.

[0032] Example 1

[0033] 5N grade antimony white (Sb 2 O 3 ) and glucose in a mass ratio of 100:15, add liquid nitrogen and ball mill for 12 hours, resonantly mix the ball-milled materials at a frequency of 80Hz and an amplitude of 2.0mm for 90 minutes, and press them into cylindrical blocks with 5mm honeycomb holes distributed inside at a pressure of 10Mpa. The blocks are placed in a vacuum furnace and heated to 300℃ for 2 hours, and then the lower end is heated to 500-1200℃ and the upper section is heated to 425℃. The lower section relies on the carbon generated by sugar to convert 5N grade antimony white (Sb 2 O 3 ) is reduced to metallic antimony, and the upper stage condenses the metallic antimony to obtain high-purity 5N metallic antimony (Sb).

[0034] When pressed into a cylindrical block with 5 mm honeycomb holes distributed inside, the mixed powder is added into a mold and pressed to obtain a block with hole distribution; the mold has 5 mm holes distributed inside, and the holes distributed in the block have a hole diameter of 5 mm.

[0035] Example 2

[0036] 5N grade antimony white (Sb 2 O 3 ) and glucose in a mass ratio of 100:25, add liquid nitrogen and ball mill for 18 hours, resonantly mix the ball milled materials at a frequency of 100Hz and an amplitude of 2.0mm for 90 minutes, and press them into cylindrical blocks with 10mm honeycomb holes distributed inside at a pressure of 10Mpa. The blocks are placed in a vacuum furnace and heated to 300℃ for 2 hours, and then the lower section is heated to 500-1200℃ and the upper section is heated to 425℃. 5N antimony white (Sb 2 O 3 ) is reduced to metallic antimony, and the upper stage condenses the metallic antimony to obtain high-purity 5N metallic antimony (Sb).

[0037] When pressed into a cylindrical block with 5mm honeycomb holes distributed inside, the mixed powder is added into a mold and pressed to obtain a block with hole distribution; the mold has a hole diameter of 10mm, and the holes distributed in the block have a hole diameter of 10mm.

[0038] Example 3

[0039] 5N grade antimony white (Sb 2 O 3 ) and glucose in a mass ratio of 100:35, add liquid nitrogen and ball mill for 24 hours, resonantly mix the ball milled materials at a frequency of 120Hz and an amplitude of 2.0mm for 90 minutes, and press them into cylindrical blocks with 20mm honeycomb holes inside at a pressure of 10Mpa. The blocks are placed in a vacuum furnace and heated to 300℃ for 2 hours, and then the lower section is heated to 500-1200℃ and the upper end is heated to 425℃. The carbon generated by glucose is used to convert 5N grade antimony white (Sb 2 O 3 ) is reduced to metallic antimony, and the metallic antimony is vacuum distilled in the upper stage to obtain high-purity 5N metallic antimony (Sb).

[0040] When pressed into a cylindrical block with 5 mm honeycomb holes distributed inside, the mixed powder is added into a mold and pressed to obtain a block with hole distribution; the mold has a hole diameter of 20 mm, and the holes distributed in the block have a hole diameter of 20 mm.

Claims

1. A method for preparing 5N grade high purity antimony metal, characterized in that Here are the steps: Step 1: Fully refine and mix glucose and antimony white to form antimony white polysaccharide mixed powder; Step 2: pressing the antimony white polysaccharide mixed powder into a porous block; Step 3: Place the porous block in a vacuum furnace and heat it, and perform high-temperature carbonization reduction at 300°C to 1000°C to reduce the 5N grade antimony white Sb2O3 to 5N grade metallic antimony.

2. The method for preparing 5N grade high purity antimony metal according to claim 1, characterized in that: The glucose and antimony white are fully refined and mixed by ball milling in a liquid nitrogen environment.

3. The method for preparing 5N grade high purity antimony metal according to claim 1, characterized in that: In step 2, the mixed powder is added into a mold and pressed to obtain a block with distributed holes; the mold has holes with a diameter of 5 to 30 mm, and the holes distributed in the block have a diameter of 5 to 30 mm.

4. The method for preparing 5N grade high purity antimony metal according to claim 2, characterized in that: The ball mill speed during the ball milling is 200r / min to 500r / min.

5. The method for preparing 5N grade high purity antimony metal according to claim 2 or 4, characterized in that: During the ball milling, the liquid nitrogen needs to cover the material, and the liquid nitrogen needs to be continuously replenished during the ball milling process.

6. The method for preparing 5N grade high purity antimony metal according to claim 1, characterized in that: The mass ratio of the 5N grade high-purity antimony white to the glucose is 100:15-35.

7. The method for preparing 5N grade high purity antimony metal according to claim 1 or 6, characterized in that: The polysaccharide is preferably glucose.

8. The method for preparing 5N grade high purity antimony metal according to claim 1, characterized in that: The heating for high-temperature carbonization reduction in step 3 adopts two heating sections, the first section is kept at room temperature to 300° C. for 2 hours, and then continues to heat up to 500-1000° C. for high-temperature carbonization.

9. The method for preparing 5N grade high purity antimony metal according to claim 8, characterized in that: The heating rate of the first stage adopts two-stage heating, starting from room temperature to 300°C for 2h, and then continuing to heat up to 400-500°C for condensation.

10. The method for preparing 5N grade high purity antimony metal according to claim 1, characterized in that: The vacuum degree of the vacuum furnace is 1x10 -4 Pa~5x10 -2 Pa.

Citation Information

Patent Citations

  • Preparation method of high-purity antimony powder

    CN116197406A

  • Preparation method of 5N-grade high-purity metal antimony

    CN116751990A