Preparation method of manganese-based multi-component alloy cast ingot
By using a combination of binary alloy, vacuum induction and self-consumption smelting in the preparation of manganese-based multi-alloy ingots, the composition inhomogeneity and processing problems in the traditional method are solved, and a high-quality and low-cost manganese-based multi-alloy is achieved. Ingot preparation, suitable for high temperature and high pressure environments of aerospace materials.
Patent Information
- Application Number
- CN202411153521.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The traditional manganese-based multi-alloy ingot preparation method has problems such as uneven composition, difficulty in processing, low processing dimensional accuracy, and unstable performance, resulting in high preparation cost and inability to improve composition uniformity.
Using binary alloys as raw materials, through the combination of vacuum induction smelting and vacuum self-consumption smelting, the fabric method, feeding sequence, smelting process and process parameters are controlled, the number of smelting times is reduced, the composition uniformity is ensured, and argon protection and AC arc stabilization are used. The current is melted to form high-quality manganese-based multi-alloy ingots.
The composition uniformity and chemical stability of manganese-based multi-alloy ingots are achieved, the total amount of impurities is reduced, the yield and welding performance are improved, and it is suitable for high-temperature and high-pressure environments of aerospace materials.
Smart Images

Figure BDA0005004257150000061 
Figure BDA0005004257150000081 
Figure BDA0005004257150000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manganese-based multi-component alloy ingot smelting, and in particular relates to a method for preparing a manganese-based multi-component alloy ingot. Background Art
[0002] As my country's aerospace industry enters a stage of rapid development, tasks such as deep space exploration, manned lunar landing, and space infrastructure construction have put forward higher requirements on the carrying capacity of rockets. As the key to ensuring the carrying capacity of heavy rockets, the design and development of a new generation of high-thrust liquid oxygen-kerosene engines is of vital importance. The structure of aerospace engines is complex. Due to the different functions and service temperatures of various parts of the engine, a variety of metal materials are often used to manufacture various parts. Due to the large differences in the performance of different metal materials, parts made of different materials cannot be directly connected during the overall manufacturing process of the engine. Instead, a type of intermediate metal is required as a transition to connect dissimilar metal parts and form a stable and strong transition layer to ensure the safety and reliability of the overall component.
[0003] Manganese can be infinitely dissolved with nickel, chromium, iron and other elements, and the bonding force between them is strong. Manganese has a high vapor pressure, low interfacial tension of its related solid solution, good wettability, and excellent gap filling ability, so it is suitable as a substrate. Manganese-based multi-element alloys have little corrosion on the base metal, so it is not easy to produce corrosion defects such as pits, undercuts or melt-through. They are mostly used in the transition connection of titanium alloys, stainless steel and high-temperature alloy parts in the aerospace field. Therefore, manganese-based multi-element alloys have become key materials for aerospace engines.
[0004] Due to the excellent performance of manganese-based multi-element alloys, manganese-based multi-element alloy ingots are mainly used in the preparation of brazing filler metals. The performance of the brazing filler metals not only affects the process performance of brazing but also determines the performance of brazed joints to a large extent. The composition (wt.) of manganese-based multi-element alloy brazing filler metals includes 30% to 45% Mn, 20% to 40% Ni and other alloying elements such as Co, Fe, Cr, Cu, etc. Traditional manganese-based multi-element alloys have overall composition deviations, and it is easy to form an intermediate brittle phase, resulting in the high brittleness of the alloy material itself, and the lack of plasticity required for rolling processing, and most of them are prepared as powder brazing filler metals.
[0005] In order to ensure the uniform melting of raw materials, the patent application number 201910525965.5, "A Cobalt-Iron-Nickel-Chromium-Manganese High Entropy Alloy Brazing Material and Its Preparation Method", carried out four smeltings; while the patent application number 202410355925.1, "A Copper-Manganese-Based Brazing Material Containing Rare Earth Components and Its Preparation Method", carried out five repeated smeltings. Excessive smelting times increase the complexity of the preparation process, resulting in a significant increase in the preparation cost, and it is impossible to further improve the composition uniformity of the manganese-based multi-element alloy. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a manganese-based multi-component alloy ingot in view of the deficiencies of the above-mentioned prior art. The method uses a binary alloy as a raw material and adopts a smelting method combining vacuum induction melting and vacuum consumable melting. By controlling the material distribution method, the order of feeding, the smelting process and the process parameters, the number of smelting times is reduced while ensuring the uniformity of the composition, and a manganese-based multi-component alloy ingot with uniform quality and chemical composition, low total impurities, stable organizational properties and high yield is prepared, which solves the problems of the manganese-based multi-component alloy ingot prepared by the traditional method, which is difficult to process, cracks in subsequent processing, low processing dimensional accuracy and unstable performance due to uneven and inaccurate composition.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a manganese-based multi-element alloy ingot, characterized in that the method comprises the following steps:
[0008] Step 1: Select binary alloy as raw material, and weigh the raw material according to the designed composition of the target product manganese-based multi-element alloy ingot;
[0009] Step 2: placing the raw materials weighed in step 1 into a crucible of a vacuum induction melting furnace according to their melting points for distribution;
[0010] Step 3, vacuum induction melting the raw materials after laying in step 2 under argon protective atmosphere, and after melting is completed, pour the melt into a water-cooled copper mold for casting and cooling to obtain a primary ingot;
[0011] Step 4: placing the primary ingot obtained in step 3 as a consumable electrode in a vacuum consumable arc furnace, performing vacuum consumable arc melting under an argon protective atmosphere, and using AC stable arc throughout the melting process to obtain a manganese-based multi-element alloy ingot.
[0012] The above-mentioned method for preparing a manganese-based multi-element alloy ingot is characterized in that the particle size of the binary alloy in step 1 is 1mm to 3mm. The present invention generally selects binary alloys such as manganese-nickel alloy, manganese-chromium alloy, copper-nickel alloy, iron-cobalt alloy as raw materials, and selects raw materials with consistent particle size, which can ensure the uniformity of the composition of the manganese-based multi-element alloy ingot prepared subsequently; at the same time, electrolytic manganese will volatilize a lot during vacuum smelting due to the low saturated vapor pressure. Selecting binary manganese-containing alloy as raw material can greatly reduce the volatilization of manganese elements during the smelting process, and ensure the uniformity and accuracy of the manganese composition in the manganese-based multi-element alloy ingot. If pure electrolytic manganese is used as raw material, the impurity content that is difficult to eliminate by smelting is significantly higher than that of binary manganese-containing alloy, thereby affecting the composition of manganese-based multi-element alloy ingot.
[0013] The above-mentioned method for preparing a manganese-based multi-element alloy ingot is characterized in that the material distribution in step 2 is: placing the raw material with a low melting point in the lower layer of the crucible, and placing the raw material with a high melting point in the upper layer of the crucible. The present invention controls the material distribution sequence, which is beneficial to the rapid melting and homogenization of the alloy elements during vacuum induction melting, and avoids the loss of low melting point raw materials.
[0014] The above-mentioned method for preparing a manganese-based multi-element alloy ingot is characterized in that the process of vacuum induction melting and casting in step 3 is as follows: after the vacuum induction melting furnace is evacuated to 0.5Pa, the power supply is gradually increased to preheat the raw materials, and the vacuum degree is kept below 5Pa. When the raw materials in the furnace are observed to be red hot, the vacuum is stopped, and argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa. At the same time, the power supply is continued to increase to start melting the raw materials. After all the raw materials are melted into a molten pool, the power supply is increased to 150kW~200kW and the smelting is continued under electromagnetic stirring. Pay attention to the degassing of the manganese-containing binary alloy in the raw materials, and keep the gas pressure in the furnace at 0.05MPa. After the smelting is completed, the smelting power is slowly reduced to half, and the surface of the molten pool forms a semi-solidified state. At this time, the manganese element will not be significantly volatilized, and the argon gas is stopped. The vacuum is continued to be evacuated until the vacuum in the furnace is 0.5Pa, and the crucible is turned over in this vacuum state for casting. Usually, the casting mold uses a water-cooled copper mold to increase the cooling speed and refine the grain.
[0015] The above-mentioned method for preparing a manganese-based multi-element alloy ingot is characterized in that the vacuum consumable arc melting process described in step four is: after evacuating the vacuum consumable arc furnace to 0.5Pa, argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa, and then arc melting is started, and argon gas is continuously filled during the melting process and an AC arc stabilizing current is used.
[0016] The present invention applies an alternating arc-stabilizing current to form a vertically upward magnetic field in a vacuum consumable arc melting furnace, thereby generating a circumferential axial force on the manganese-based multi-component alloy melt, thereby fully stirring the melt as a whole, promoting uniform temperature distribution of the melt, and eliminating obvious temperature gradients in all directions, which is beneficial to equiaxed crystal growth, increases the nucleation rate of grains, reduces metallurgical defects caused by uneven composition, and improves the composition uniformity of manganese-based multi-component alloy ingots.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] 1. The present invention studies the burning law of the volatile element Mn during smelting, and adopts binary alloys including manganese-containing binary alloys as raw materials. Since the manganese element in the manganese-containing binary alloy has been alloyed, the burning and volatilization amount of manganese during the smelting process is significantly reduced, thereby improving the uniformity and accuracy of the manganese content in the product ingot; at the same time, the binary alloy raw material used combines the melting point difference and density difference between the elements, thereby avoiding the problems of element burning caused by the melting point difference and the uneven composition caused by the density difference during the smelting process, thereby improving the uniformity and stability of the content of each element in the manganese-based multi-element alloy ingot, and the preparation process is the simplest and easy to produce.
[0019] 2. Compared with the conventional manganese-based multi-element alloy smelting which often uses single metal raw materials, resulting in poor overall uniformity of the ingot and easy segregation or inclusion, the present invention uses binary alloy as raw material to improve the overall uniformity of the manganese-based multi-element alloy ingot, and effectively avoids the ingot segregation problem caused by uneven mixing of single raw materials or excessive difference in melting point during the smelting process.
[0020] 3. The binary alloy used in the present invention has been homogenized as a whole, so it can be used as a raw material in the subsequent ingot preparation process to better produce titanium alloy ingots with uniform composition, small segregation, low impurity content and good overall quality. At the same time, the use of binary alloys can reduce the number of smelting times in the preparation process of manganese-based multi-component alloys, significantly saving costs.
[0021] 4. The present invention adopts vacuum induction melting combined with water-cooled copper mold forming, and argon gas protection is filled in the vacuum induction melting process, which greatly reduces the burn-in of the Mn element. The vacuum induction melting ensures that all raw materials are completely melted, and the water-cooled copper mold helps to quickly form the melt with almost no loss, further improving the uniformity and stability of the content of each element in the manganese-based multi-element alloy ingot.
[0022] 5. The present invention adopts vacuum consumable arc melting, and the entire melting process uses AC stable arc, so that the molten pool rotates during the melting process, ensuring the uniformity of the manganese-based multi-element alloy ingot; at the same time, the use of vacuum consumable arc melting can be used for shrinkage compensation, reducing the shrinkage cavity and looseness of the ingot, so that the defects are completely retained in the ingot riser, thereby improving the yield of the manganese-based multi-element alloy ingot.
[0023] 6. The present invention adopts a smelting method of vacuum induction melting combined with vacuum consumable melting, which can significantly reduce the number of ingot melting times while ensuring the overall uniformity of the composition of the manganese-based multi-component alloy ingot. Both methods are argon-filled melting, which can well control the burning loss of the manganese-based multi-component alloy. At the same time, the combination of the two melting methods improves the yield of the multi-component alloy ingot.
[0024] 7. The manganese-based multi-element alloy ingot prepared by the present invention has uniform quality, stable chemical composition, low total impurities, good welding performance, superior process performance, high yield, and is not prone to cracking in subsequent strip processing. It is suitable for preparing manganese-based multi-element alloy brazing materials for aerospace materials, and the use temperature of the weld after welding with the solder can reach 1150°C, and the tensile strength can reach more than 1000MPa. It has good performance in high temperature, high pressure and liquid oxygen environment.
[0025] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION
[0026] Example 1
[0027] This embodiment includes the following steps:
[0028] Step 1: Select manganese-nickel alloy, manganese-chromium alloy and iron-cobalt alloy with a particle size of 1 mm to 3 mm as raw materials, and weigh the raw materials according to the designed composition of the target product manganese-based multi-element alloy ingot Mn-35Ni-11.5Cr-1.5Fe-1.8Co (wt%);
[0029] Step 2: Place the manganese-nickel alloy, manganese-chromium alloy, and iron-cobalt alloy raw materials weighed in step 1 into a crucible of a vacuum induction melting furnace according to their melting points: place the manganese-nickel alloy in the lower layer of the crucible, and place the manganese-chromium alloy and iron-cobalt alloy in the upper layer of the crucible.
[0030] Step 3, after the vacuum induction melting furnace after the material is laid in step 2 is evacuated to 0.5Pa, the power supply is gradually increased to preheat the raw materials, and the vacuum degree is kept below 5Pa. When the raw materials in the furnace are observed to be red hot, the vacuum is stopped, and argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa. At the same time, the power supply is continued to increase to start melting the raw materials. After all the raw materials are melted into a molten pool, the power supply is increased to 150kW~200kW and the smelting is continued under electromagnetic stirring. Pay attention to the degassing of manganese-nickel alloy and manganese-chromium alloy in the raw materials, and keep the gas pressure in the furnace at 0.05MPa. After the smelting is completed, the smelting power is slowly reduced to half, and the surface of the molten pool forms a semi-solidified state. At this time, the manganese element will not be obviously volatilized, and the argon gas is stopped. The vacuum is continued to be evacuated until the vacuum in the furnace is 0.5Pa, and the crucible is turned over in the vacuum state for casting. The casting mold uses a water-cooled copper mold, and the mold is demolded after cooling for 2 hours to obtain a primary ingot;
[0031] Step 4. Place the primary ingot obtained in step 3 as a consumable electrode in a vacuum consumable arc furnace. After evacuating the vacuum consumable arc furnace to 0.5 Pa, fill the vacuum chamber with argon gas with a mass purity of 99.999% to make the pressure in the furnace reach 0.05 MPa, and then start arc melting. During the melting process, argon gas is continuously filled and an AC arc stabilizing current is used. During the melting process, the current is 4kA~8kA, the voltage is 28V~32V, and the AC arc stabilizing current is 6A. After 2 hours after the melting is completed, the ingot is taken out of the furnace to obtain a manganese-based multi-element alloy ingot.
[0032] The manganese-based multi-element alloy ingot prepared in this embodiment was flattened and peeled on a lathe, and samples were taken from the upper, middle and lower parts of the ingot for block testing of chemical composition. The results are shown in Table 1 below.
[0033] Table 1
[0034]
[0035] It can be seen from Table 1 that the absolute value of the composition fluctuation deviation of the upper, middle and lower parts of the manganese-based multi-component alloy ingot prepared in this embodiment is less than 1%, the uniformity of each alloy component is good, and there are no defects such as inclusions in the manganese-based multi-component alloy ingot, which meets the requirements of large-scale industrial production for the uniformity of composition distribution of manganese-based multi-component alloy ingots.
[0036] Example 2
[0037] This embodiment includes the following steps:
[0038] Step 1: Select manganese-nickel alloy and manganese-chromium alloy as raw materials, and weigh the raw materials according to the designed composition Mn-26Ni-5Cr (wt%) of the target product manganese-based multi-element alloy ingot;
[0039] Step 2: placing the manganese-nickel alloy and manganese-chromium alloy raw materials weighed in step 1 into a crucible of a vacuum induction melting furnace according to their melting points for distribution: placing the manganese-nickel alloy in the lower layer of the crucible, and placing the manganese-chromium alloy in the upper layer of the crucible;
[0040] Step 3, after the vacuum induction melting furnace after the material is laid in step 2 is evacuated to 0.5Pa, the power supply is gradually increased to preheat the raw materials, and the vacuum degree is kept below 5Pa. When the raw materials in the furnace are observed to be red hot, the vacuum is stopped, and argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa. At the same time, the power supply is continued to increase to start melting the raw materials. After all the raw materials are melted into a molten pool, the power supply is increased to 150kW~200kW and the smelting is continued under electromagnetic stirring. Pay attention to the degassing of manganese-nickel alloy and manganese-chromium alloy in the raw materials, and keep the gas pressure in the furnace at 0.05MPa. After the smelting is completed, the smelting power is slowly reduced to half, and the surface of the molten pool forms a semi-solidified state. At this time, the manganese element will not be obviously volatilized, and the argon gas is stopped. The vacuum is continued to be evacuated until the vacuum in the furnace is 0.5Pa, and the crucible is turned over in the vacuum state for casting. The casting mold uses a water-cooled copper mold, and the mold is demolded after cooling for 2 hours to obtain a primary ingot;
[0041] Step 4. Place the primary ingot obtained in step 3 as a consumable electrode in a vacuum consumable arc furnace. After evacuating the vacuum consumable arc furnace to 0.5 Pa, fill the vacuum chamber with argon gas with a mass purity of 99.999% to make the pressure in the furnace reach 0.05 MPa, and then start arc melting. During the melting process, argon gas is continuously filled and an AC arc stabilizing current is used. During the melting process, the current is 4kA~8kA, the voltage is 28V~32V, and the AC arc stabilizing current is 6A. After 2 hours after the melting is completed, the ingot is taken out of the furnace to obtain a manganese-based multi-element alloy ingot.
[0042] The manganese-based multi-element alloy ingot prepared in this embodiment was flattened and peeled on a lathe, and samples were taken from the upper, middle and lower parts of the ingot for block testing of chemical composition. The results are shown in Table 2 below.
[0043] Table 2
[0044]
[0045] It can be seen from Table 2 that the absolute value of the composition fluctuation deviation of the upper, middle and lower parts of the manganese-based multi-component alloy ingot prepared in this embodiment is less than 1%, the uniformity of each alloy component is good, and there are no defects such as inclusions in the manganese-based multi-component alloy ingot, which meets the requirements of large-scale industrial production for the uniformity of composition distribution of manganese-based multi-component alloy ingots.
[0046] Example 3
[0047] This embodiment includes the following steps:
[0048] Step 1: Select manganese-nickel alloy, manganese-chromium alloy, and copper-nickel alloy as raw materials, and weigh the raw materials according to the designed composition Mn-36Ni-12Cr-3.5Cu (wt%) of the target product manganese-based multi-element alloy ingot;
[0049] Step 2: placing the manganese-nickel alloy, manganese-chromium alloy, and copper-nickel alloy raw materials weighed in step 1 into a crucible of a vacuum induction melting furnace according to their melting points for distribution: placing the manganese-nickel alloy in the lower layer of the crucible, and placing the manganese-chromium alloy and copper-nickel alloy in the upper layer of the crucible;
[0050] Step 3, after the vacuum induction melting furnace after the material is laid in step 2 is evacuated to 0.5Pa, the power supply is gradually increased to preheat the raw materials, and the vacuum degree is kept below 5Pa. When the raw materials in the furnace are observed to be red hot, the vacuum is stopped, and argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa. At the same time, the power supply is continued to increase to start melting the raw materials. After all the raw materials are melted into a molten pool, the power supply is increased to 150kW~200kW and the smelting is continued under electromagnetic stirring. Pay attention to the degassing of manganese-nickel alloy and manganese-chromium alloy in the raw materials, and keep the gas pressure in the furnace at 0.05MPa. After the smelting is completed, the smelting power is slowly reduced to half, and the surface of the molten pool forms a semi-solidified state. At this time, the manganese element will not be obviously volatilized, and the argon gas is stopped. The vacuum is continued to be evacuated until the vacuum in the furnace is 0.5Pa, and the crucible is turned over in the vacuum state for casting. The casting mold uses a water-cooled copper mold, and the mold is demolded after cooling for 2 hours to obtain a primary ingot;
[0051] Step 4. Place the primary ingot obtained in step 3 as a consumable electrode in a vacuum consumable arc furnace. After evacuating the vacuum consumable arc furnace to 0.5 Pa, fill the vacuum chamber with argon gas with a mass purity of 99.999% to make the pressure in the furnace reach 0.05 MPa, and then start arc melting. During the melting process, argon gas is continuously filled and an AC arc stabilizing current is used. During the melting process, the current is 4kA~8kA, the voltage is 28V~32V, and the AC arc stabilizing current is 6A. After 2 hours after the melting is completed, the ingot is taken out of the furnace to obtain a manganese-based multi-element alloy ingot.
[0052] The manganese-based multi-element alloy ingot prepared in this embodiment was flattened and peeled on a lathe, and samples were taken from the upper, middle and lower parts of the ingot for block testing of chemical composition. The results are shown in Table 3 below.
[0053] Table 3
[0054]
[0055] It can be seen from Table 3 that the absolute value of the composition fluctuation deviation of the upper, middle and lower parts of the manganese-based multi-component alloy ingot prepared in this embodiment is less than 1%, the uniformity of each alloy component is good, and there are no defects such as inclusions in the manganese-based multi-component alloy ingot, which meets the requirements of large-scale industrial production for the uniformity of composition distribution of manganese-based multi-component alloy ingots.
[0056] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a manganese-based multi-element alloy ingot, characterized in that: The method comprises the following steps: Step 1: Select binary alloy as raw material, and weigh the raw material according to the designed component composition of the target product manganese-based multi-element alloy ingot; Step 2: placing the raw materials weighed in step 1 into a crucible of a vacuum induction melting furnace according to their melting points for distribution; Step 3, vacuum induction melting the raw materials after laying in step 2 under argon protective atmosphere, and after melting is completed, pour the melt into a water-cooled copper mold for casting and cooling to obtain a primary ingot; Step 4: placing the primary ingot obtained in step 3 as a consumable electrode in a vacuum consumable arc furnace, performing vacuum consumable arc melting under an argon protective atmosphere, and using AC stable arc throughout the melting process to obtain a manganese-based multi-element alloy ingot.
2. The method for preparing a manganese-based multi-element alloy ingot according to claim 1, characterized in that: The particle size of the binary alloy in step 1 is 1 mm to 3 mm.
3. The method for preparing a manganese-based multi-element alloy ingot according to claim 1, characterized in that: The distribution in step 2 is as follows: placing the raw material with a low melting point in the lower layer of the crucible, and placing the raw material with a high melting point in the upper layer of the crucible.
4. The method for preparing a manganese-based multi-element alloy ingot according to claim 1, characterized in that: The process of vacuum induction melting and casting described in step 3 is as follows: after the vacuum induction melting furnace is evacuated to 0.5Pa, the power supply is gradually increased to preheat the raw materials, and the vacuum degree is kept below 5Pa. When the raw materials in the furnace are observed to be red hot, the vacuum is stopped, and argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa. At the same time, the power supply is continued to increase to start melting the raw materials. After all the raw materials are melted into a molten pool, the power supply is increased to 150kW~200kW and the melting is continued under electromagnetic stirring. Pay attention to the degassing of the manganese binary alloy in the raw materials, and keep the gas pressure in the furnace at 0.05MPa. After the melting is completed, the melting power is slowly reduced to half, and the surface of the molten pool forms a semi-solidified state. At this time, the manganese element will not be obviously volatilized, and the argon gas is stopped. The vacuum is continued to be evacuated until the vacuum in the furnace is 0.5Pa, and the crucible is turned over in this vacuum state for casting.
5. The method for preparing a manganese-based multi-element alloy ingot according to claim 1, characterized in that: The process of vacuum consumable arc melting described in step 4 is: after evacuating the vacuum consumable arc furnace to 0.5Pa, argon gas with a mass purity of 99.999% is filled into the vacuum chamber to make the pressure in the furnace reach 0.05MPa, and then arc melting is started, and argon gas is continuously filled during the melting process and an AC arc stabilizing current is used.
Citation Information
Cited By
Non-vacuum melting preparation method of Mn-based alloy
CN121450974A