Sn / Mg microalloyed ultrahigh-strength conductive copper-titanium alloy and preparation method thereof

Through Sn/Mg microalloyation and multi-stage thermal mechanical treatment, CuSn3Ti5 phase and α-Cu4Ti precipitation phase are formed, solving the problem of low conductivity of copper-titanium alloys and achieving comprehensive performance improvements of high strength and high conductivity.

CN119020632AActive Publication Date: 2024-11-26TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411071509.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing copper-titanium alloys are not ideal in terms of strength and conductivity of the balanced material, and it is difficult to improve the conductivity while ensuring high strength.

Method used

Through Sn/Mg microalloyization, multi-stage thermal mechanical treatment methods are adopted, including vacuum induction smelting, hot rolling, solid solution treatment, cold rolling and aging treatment, to form CuSn3Ti5 phase and α-Cu4Ti precipitation phase, and improve the conductivity of the alloy and strength.

Benefits of technology

The high strength and high conductivity of copper-titanium alloys are achieved, with hardness ≥300HV, conductivity ≥26% IACS, tensile strength ≥1000MPa, and the overall performance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020632A_ABST
    Figure CN119020632A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of beryllium-free copper alloy materials, in particular to Sn / Mg microalloyed ultrahigh-strength conductive copper-titanium alloy and a preparation method thereof. The Sn / Mg microalloyed ultrahigh-strength conductive copper-titanium alloy comprises the following elements: 2-5% of Ti, 0.1-3% of Sn, 0.1-3% of Mg and the balance of Cu and inevitable impurities, and the Sn / Mg microalloyed ultrahigh-strength conductive copper-titanium alloy has the hardness of more than or equal to 300HV, the conductivity of more than or equal to 26% IACS (International Annealed Copper Standard), the tensile strength of more than or equal to 1000MPa, outstanding comprehensive performance, high strength and high conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of beryllium-free copper alloy materials, and in particular to a Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy and a preparation method thereof. Background Art

[0002] Copper-beryllium alloys are widely used in electronic components, various precision instruments, etc. due to their high strength and good conductivity. However, after fully realizing the serious harm of copper-beryllium alloys in production to health and the environment, people began to seek alternative materials to beryllium bronze.

[0003] Copper-titanium alloy is a typical precipitation hardening alloy, and its mechanical properties are comparable to those of copper-beryllium alloy, but its electrical conductivity is lower than that of copper-beryllium alloy. In order to improve the electrical conductivity of copper-titanium alloy while ensuring its mechanical properties, the prior art proposes to add different trace elements and plastic deformation and heat treatment to synergize to improve material properties, such as patent CN202110203008.8 discloses a copper-titanium alloy with high strength and high plasticity requirements and bending and its preparation method, patent CN201910261814.3 discloses a copper-titanium alloy with high hardness, high toughness, good brittleness and thermal conductivity and its preparation method, and patent CN202010620874.2 discloses a copper-titanium alloy with high strength and high plasticity and its preparation method. However, the above patents are not ideal in balancing the strength and electrical conductivity of the material. Therefore, there is an urgent need for a method that can ensure the high strength of copper-titanium alloy while improving its electrical conductivity. Summary of the invention

[0004] The object of the present invention is to provide a Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy, which has high strength and high conductivity.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] A Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy, the element composition of which includes Ti2-5%, Sn 0.1-3%, Mg 0.1-3%, and the balance is Cu and unavoidable impurities.

[0007] The preparation method of the conductive copper-titanium alloy comprises the following steps:

[0008] S1 prepares raw materials and vacuum induction melts Cu-Ti-Mg-Sn alloy ingots;

[0009] S2 performs multiple hot rolling treatments on the cast alloy at a holding temperature of 650-750°C, with a deformation of 50-70%, and air cooling after the hot rolling is completed; S3 performs a heat preservation solid solution treatment on the hot rolled alloy plate at 750-850°C, and water cooling at room temperature; after the solid solution treatment is completed, the first cold rolling is performed, with a cold rolling deformation of 50-70%, to obtain a copper-titanium alloy plate;

[0010] After cold rolling, CuSn3Ti5 phase appears, which improves the electrical conductivity of the alloy; defects introduced by cold rolling, such as dislocations, provide driving force for subsequent aging precipitation;

[0011] S4: aging the copper-titanium alloy plate at 380°C ± 10°C for 0.5 to 100 hours, followed by air cooling;

[0012] S5 performs a second cold rolling on the alloy, with a cold rolling deformation of 50 to 70%;

[0013] S6: The alloy obtained by the second cold rolling is subjected to aging treatment at 350°C±10°C for 0.5 to 100 hours to obtain an ultra-high strength conductive copper-titanium alloy.

[0014] In S4 of the method for preparing the Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy of the present invention, it has been verified by experiments that when the aging time is short, the strength is the best, but the conductivity is not high; with the extension of the aging time, the hardness, strength and conductivity are significantly improved. The possible reason is that the number of precipitated phases increases with the extension of the aging time, and the size becomes larger. Specifically, the precipitation of the CuSn3Ti5 phase increases, the Mg element is evenly distributed in the copper matrix, and the α-Cu4Ti phase is dispersed and precipitated. The material obtained after the second cold rolling was tested and the hardness and strength were improved. The hardness increased to 300HV, the tensile strength increased to 1050MPa, and the conductivity only decreased slightly, still maintaining a high conductivity of 21%IACS.

[0015] Preferably, S1 is: according to the formula, first add Cu into a vacuum induction furnace for melting, the melting temperature is 1250℃±50℃, add Ti after filling with argon, stir thoroughly, and after refining for 20-25 minutes, add Sn and Mg to the melt in sequence, stir thoroughly and then cast, the casting temperature is 1150℃±50℃.

[0016] Preferably, the hot rolling is carried out at a holding temperature of 720°C to 740°C in S2 for 2.5 to 3.5 hours, and the deformation is 60% to 65%. More preferably, the hot rolling is carried out at a holding temperature of 730°C for 3 hours, and the deformation is 60%.

[0017] Preferably, the hot-rolled alloy plate in S3 is solution treated at 780-800°C and kept warm for 3-4 hours.

[0018] Preferably, the deformation amount of the first cold rolling in S3 is 55-65%.

[0019] Preferably, the deformation amount of the second cold rolling in S5 is 50 to 55%.

[0020] Preferably, the aging treatment time of S4 and S6 is 90h to 100h. The best aging parameter after the first cold rolling is aging at 380°C for 100h, and the best aging parameter after the second cold rolling is aging at 350°C for 100h.

[0021] Preferably, the conductive copper-titanium alloy comprises 3% Ti, 0.5-1% Sn, 0.5% Mg, and the remainder is Cu and inevitable impurities.

[0022] A method for preparing a Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy, the method comprising the following steps:

[0023] S1 prepares raw materials and vacuum induction melts Cu-Ti-Mg-Sn alloy ingots;

[0024] S2 performs multiple hot rolling treatments on the cast alloy at a holding temperature of 650-750°C, with a deformation of 50-70%, and air cooling after the hot rolling is completed; S3 performs a heat preservation solid solution treatment on the hot rolled alloy plate at 750-850°C, and water cooling at room temperature; after the solid solution treatment is completed, the first cold rolling is performed, with a cold rolling deformation of 50-70%, to obtain a copper-titanium alloy plate;

[0025] After cold rolling, CuSn3Ti5 intermetallic compounds appear, which improve the electrical conductivity of the alloy; defects introduced by cold rolling, such as dislocations, provide driving force for subsequent aging precipitation;

[0026] S4: aging treatment of the copper-titanium alloy plate at 380°C ± 10°C for 0.5 to 100 h, followed by water quenching at room temperature;

[0027] S5 performs a second cold rolling on the alloy, with a cold rolling deformation of 50 to 70%;

[0028] S6: The alloy obtained by the second cold rolling is subjected to aging treatment at 350°C±10°C for 0.5 to 100 hours to obtain an ultra-high strength conductive copper-titanium alloy.

[0029] The beneficial effects of the present invention are:

[0030] On the basis of binary Cu-Ti alloy, the present invention improves the strength and conductivity of Cu-Ti alloy by adding alloying elements combined with multi-stage thermomechanical treatment. The Mg element is dissolved in the matrix to play a role of solid solution strengthening; Sn and Ti can form CuSn3Ti5 phase during the aging process, which reduces the content of solid solution Ti and improves the conductivity of the alloy; at the same time, during the aging process, the volume fraction of α-Cu4Ti precipitation phase is increased, thereby further improving the strength and conductivity of the alloy. The Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy of the present invention has a hardness of ≥300HV, a conductivity of ≥26%IACS, a tensile strength of ≥1000MPa, outstanding comprehensive performance, and high strength and high conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 These are the metallographic images of (a) Cu-3Ti alloy (b) Cu-3Ti-0.5Mg-0.5Sn alloy (c) Cu-3Ti-0.5Mg-1Sn alloy;

[0032] Figure 2 It is the hardness and conductivity curve of Cu-3Ti-0.5Mg-0.5Sn alloy after single cold rolling + aging;

[0033] Figure 3 It is the XRD spectrum of Cu-3Ti-0.5Mg-0.5Sn alloy after one cold rolling and aging at 380℃ for different time;

[0034] Figure 4 It is the TEM image of Cu-3Ti-0.5Mg-0.5Sn alloy after primary cold rolling and aging at 380℃ for 100h;

[0035] Figure 5 It is the hardness and conductivity curve of Cu-3Ti-0.5Mg-0.5Sn alloy after secondary cold rolling + aging;

[0036] Figure 6 The transmission electron microscopy (TEM) images and the selected area electron diffraction (SAED) images of Cu-3Ti-0.5Mg-0.5Sn alloy aged at 350℃ for (a) 2h; (c) 100h and (b) 2h; (d) 100h after secondary cold rolling.

[0037] Figure 7 It is the stress-strain curve of Cu-3Ti-0.5Mg-0.5Sn alloy and Cu-3Ti-0.5Mg-1Sn alloy after secondary cold rolling + aging;

[0038] Figure 8 It is the hardness and conductivity curve of Cu-3Ti-0.5Mg-1Sn alloy after secondary cold rolling + aging. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.

[0040] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0041] Unless otherwise specified, the reagents used in the following examples can be purchased from conventional biochemical reagent stores.

[0042] The core of the present invention is to provide a Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy, the element composition of the conductive copper-titanium alloy includes Ti 2-5%, Sn 0.1-3%, Mg 0.1-3%, and the balance is Cu and inevitable impurities. The preparation method of the conductive copper-titanium alloy includes the following steps:

[0043] S1 prepares raw materials and vacuum induction melts Cu-Ti-Mg-Sn alloy ingots;

[0044] S2: subjecting the as-cast alloy to a multi-pass hot rolling treatment at a holding temperature of 650-750°C, with a deformation amount of 50-70%, and air cooling after the hot rolling is completed;

[0045] S3 performs a heat preservation solid solution treatment on the hot-rolled alloy plate at 750-850°C, and water-cools at room temperature; after the solid solution treatment is completed, the first cold rolling is performed, and the cold rolling deformation is 50-70%, so as to obtain a copper-titanium alloy plate;

[0046] S4: aging the copper-titanium alloy plate at 380°C ± 10°C for 0.5 to 100 hours, followed by air cooling;

[0047] S5 performs a second cold rolling on the alloy, with a cold rolling deformation of 50 to 70%;

[0048] S6: The alloy obtained by the second cold rolling is subjected to aging treatment at 350°C±10°C for 0.5 to 100 hours to obtain an ultra-high strength conductive copper-titanium alloy.

[0049] The optimal element composition of the conductive copper-titanium alloy includes 3% Ti, 0.5-1% Sn, 0.5% Mg, and the balance is Cu and inevitable impurities.

[0050] The best aging parameters after the first cold rolling are 380℃ for 100h, and the best aging parameters after the second cold rolling are 350℃ for 100h.

[0051] Example 1

[0052] Calculated by mass percentage, the composition of the Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy is: Ti 3%, Sn 0.5%, Mg 0.5%, and the balance is copper.

[0053] Preparation method of the Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy:

[0054] (1) First, Cu is added into a vacuum induction furnace for smelting at a smelting temperature of 1250°C, and Ti is added after filling with argon gas, and fully stirred. After refining for 20 minutes, Sn and Mg are added to the melt in sequence, and after fully stirring, casting is performed at a casting temperature of 1150°C, and a copper-titanium alloy ingot is obtained after surface milling;

[0055] The ingot was milled to remove surface defects, and its hardness was measured to be about 310 HV and its conductivity was 9.0% IACS, which is about 50 HV higher than that of Cu-3Ti binary cast alloy.

[0056] Metallographic images of (a) Cu-3Ti alloy (b) Cu-3Ti-0.5Mg-0.5Sn alloy (c) Cu-3Ti-0.5Mg-1Sn alloy are shown in Figure 1 Through the observation of the metallographic structure of the cast alloy, it was found that the dendrite spacing of the multi-component cast alloy was smaller than that of the Cu-3Ti binary alloy, which provided evidence for the improvement of the strength of the cast alloy. Figure 1 shown.

[0057] (2) hot rolling the copper-titanium alloy ingot obtained in step (1) at 730° C., keeping the temperature for 3 h, and deforming the ingot by 60%; then performing a solid solution treatment at 800° C., keeping the temperature for 4 h, water cooling at room temperature, and then performing a first cold rolling at room temperature, with a deformation of 60%, to obtain a copper-titanium alloy plate;

[0058] After cold rolling, CuSn3Ti5 phase appeared, which improved the electrical conductivity of the alloy ( Figure 3 , Figure 4 ). Defects introduced by cold rolling, such as dislocations, provide driving force for subsequent aging precipitation ( Figure 4 ).

[0059] (3) subjecting the copper-titanium alloy plate obtained in step (2) to aging treatment at 380° C. for 100 h, and cooling with air;

[0060] from Figure 2It can be seen that the hardness and conductivity of the single cold rolling + aging vary greatly with the change of aging temperature. The hardness of the sample first increases and then decreases with the aging time. The higher the aging temperature, the shorter the time to reach the peak hardness. The hardness of the samples aged at 500℃ for 0.5h, 450℃ for 0.5h, and 380℃ for 1h all reached peak values ​​of 310HV, 340HV, and 337HV, respectively. As the aging time increases, the higher the aging temperature, the faster the hardness decreases. The conductivity of the sample gradually increases with the extension of the aging time. In the early stage of aging, the higher the aging temperature, the faster the conductivity increases. In the later stage of aging, the conductivity of the sample increases slowly. After aging at 380℃ for 100h, the conductivity of the sample reached 22.3%IACS. After aging at 450℃ for 100h, the conductivity of the sample reached 21.2%IACS. Considering the hardness and conductivity, the best aging parameter after single cold rolling is aging at 380℃ for 100h.

[0061] from Figure 3 It can be seen that CuSn3Ti5 phase appears in the sample after cold rolling. With the extension of aging time, in addition to CuSn3Ti5 phase, Cu2Mg phase also appears in the alloy.

[0062] Figure 4 Submicron-sized CuSn3Ti5 phases can be observed in the precipitate, and dislocations are present. The appearance of dislocations provides a driving force for the formation of precipitated phases.

[0063] (4) then performing a second cold rolling at room temperature, wherein the deformation amount of the second cold rolling is 50%, to obtain a second cold rolled copper-titanium alloy plate;

[0064] After the cold rolling, the hardness and strength were improved, the hardness increased to 300 HV, the tensile strength increased to 1050 MPa, and the conductivity only decreased slightly, still maintaining a high conductivity of 21% IACS. (4) The second cold-rolled copper-titanium alloy plate obtained in step (3) was kept at 350° C. for 100 h and air-cooled to obtain an ultra-high strength conductive copper-titanium alloy.

[0065] from Figure 5 It can be seen that the hardness of the samples aged at 350℃ and 380℃ after secondary cold rolling remains basically unchanged with the aging time, and the conductivity gradually increases. The hardness values ​​of the two aging temperatures are not much different, but the conductivity of the samples aged at 350℃ is better than that of the samples aged at 380℃. The aging parameters with the best comprehensive performance are aging at 350℃ for 100h.

[0066] from Figure 6 It can be seen that after the second cold rolling and aging at 350℃ for 2h, a large number of nano-scale α-Cu4Ti precipitates appeared in the sample. And after aging for 100h, the number of α-Cu4Ti precipitates increased. The corresponding SAED graph confirmed the existence of α-Cu4Ti precipitates. The α-Cu4Ti precipitates increased the strength of the alloy, which was greater than 800MPa. Figure 7 shown.

[0067] Example 2

[0068] The composition of the Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy is, in terms of mass percentage, 3% Ti, 1% Sn, 0.5% Mg, and the balance is copper. The preparation method of the Sn / Mg microalloyed ultra-high-strength conductive copper-titanium alloy is the same as that of Example 1.

[0069] The hardness and conductivity curves of Cu-3Ti-0.5Mg-0.5Sn alloy (Example 1) and Cu-3Ti-0.5Mg-1Sn alloy (Example 2) after secondary cold rolling + aging are as follows: Figure 2 As shown; the stress-strain curves of Cu-3Ti-0.5Mg-0.5Sn alloy and Cu-3Ti-0.5Mg-1Sn alloy after secondary cold rolling + aging are shown in Figure 3 As shown. Figure 5 , Figure 7 and Figure 8 It can be seen that after secondary cold rolling + aging, the hardness of the alloy is basically maintained at 310HV, the strength is greater than 800MPa, and the conductivity gradually increases. After secondary cold rolling + aging at 350℃ for 100h, the comprehensive performance of the alloy is the best, with a strength greater than 1100MPa and a conductivity greater than 25%IACS.

[0070] Comparative Examples 1 to 6

[0071] Conductive copper-titanium alloys with different element compositions were prepared using the same preparation method as in Example 1 to compare the effects of each component on the properties of the copper-titanium alloy.

[0072] The components of the copper-titanium alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 6 were tested. The test results are shown in Table 1.

[0073] Table 1 Composition of copper-titanium alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 6

[0074]

[0075]

[0076] The hardness, tensile strength, electrical conductivity and elongation of the copper-titanium alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 6 were tested. The test results are shown in Table 2.

[0077] The testing methods for hardness, tensile strength, elongation and conductivity are based on GB / T 4340.1-2009, GB / T228.1-2010 and JB / T 13940-2020 respectively.

[0078] Table 2 Hardness, tensile strength, conductivity and elongation of copper-titanium alloy

[0079]

[0080] It can be seen from the data in Table 2 that the ultra-high strength conductive copper-titanium alloy prepared by the preparation method provided by the present invention has high strength and high conductivity. The hardness of the alloy prepared in Example 1 can reach 310HV, the tensile strength can reach 1150MPa, and the conductivity can reach more than 25%IACS, and the performance is relatively outstanding.

[0081] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0082] The above is a detailed introduction to a Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy, Features: The element composition of the conductive copper-titanium alloy includes 2-5% Ti, 0.1-3% Sn, 0.1-3% Mg, and the balance is Cu and inevitable impurities; The preparation method of the conductive copper-titanium alloy comprises the following steps: S1 prepares raw materials and vacuum induction melts Cu-Ti-Mg-Sn alloy ingots; S2: subjecting the as-cast alloy to a multi-pass hot rolling treatment at a holding temperature of 650-750°C, with a deformation amount of 50-70%, and air cooling after the hot rolling is completed; S3 performs a heat preservation solid solution treatment on the hot-rolled alloy plate at 750-850°C, and water-cools at room temperature; after the solid solution treatment is completed, the first cold rolling is performed, and the cold rolling deformation is 50-70%, so as to obtain a copper-titanium alloy plate; S4: aging the copper-titanium alloy plate at 380°C ± 10°C for 0.5 to 100 hours, followed by air cooling; S5 performs a second cold rolling on the alloy, with a cold rolling deformation of 50 to 70%; S6: The alloy obtained by the second cold rolling is subjected to aging treatment at 350°C±10°C for 0.5 to 100 hours to obtain an ultra-high strength conductive copper-titanium alloy.

2. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: S1 is: according to the formula, first add Cu into the vacuum induction furnace for melting, the melting temperature is 1250℃±50℃, fill with argon gas and add Ti, stir well, refine for 20-25 minutes, then add Sn and Mg to the melt in turn, stir well and then cast, the casting temperature is 1150℃±50℃.

3. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: In S2, the hot rolling is carried out at a holding temperature of 720°C to 740°C for 2.5 to 3.5 hours, and the deformation amount is 60% to 65%.

4. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: In S3, the hot-rolled alloy plate is solution treated at 780-800°C and kept warm for 3-4h.

5. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: The deformation amount of the first cold rolling of S3 is 55-65%.

6. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: The deformation amount of the second cold rolling in S5 is 50-55%.

7. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: The aging treatment time of S4 and S6 is 90h~100h.

8. The Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy according to claim 1, Features: The element composition of the conductive copper-titanium alloy includes 3% Ti, 0.5-1% Sn, 0.5% Mg, and the balance is Cu and inevitable impurities.

9. A method for preparing a Sn / Mg microalloyed ultra-high strength conductive copper-titanium alloy. Features The preparation method of the conductive copper-titanium alloy comprises the following steps: S1 prepares raw materials and vacuum induction melts Cu-Ti-Mg-Sn alloy ingots; S2 performs multiple hot rolling treatments on the cast alloy at a holding temperature of 650-750°C, with a deformation of 50-70%, and air cooling after the hot rolling is completed; S3 performs a heat preservation solid solution treatment on the hot rolled alloy plate at 750-850°C, and water cooling at room temperature; after the solid solution treatment is completed, the first cold rolling is performed, with a cold rolling deformation of 50-70%, to obtain a copper-titanium alloy plate; S4: aging the copper-titanium alloy plate at 380°C ± 10°C for 0.5 to 100 hours, followed by air cooling; S5 performs a second cold rolling on the alloy, with a cold rolling deformation of 50 to 70%; S6: The alloy obtained by the second cold rolling is subjected to aging treatment at 350°C±10°C for 0.5 to 100 hours to obtain an ultra-high strength conductive copper-titanium alloy.

Citation Information

Patent Citations

  • Rare earth titanium-copper alloy and manufacture method thereof

    CN101144128A

  • Preparation method of tin-copper alloy bar

    CN104561645A

  • High-strength and high-elasticity conductive Cu-Ti alloy strip and preparation method thereof

    CN110747363A

  • Method for simultaneously improving strength and electric conductivity of Cu-Cr-Nb alloy

    CN112553500A

  • Copper-titanium alloy and preparation method thereof

    CN113005324A