Low-temperature high-strength and high-toughness cast steel for ships and preparation method thereof
By controlling the types and content of elements, combining secondary normalization and primary tempering processes, the microstructure of marine cast steel is improved, and the problem of insufficient low-temperature toughness at -40℃ in the existing technology is solved, and the problem of insufficient low-temperature toughness at -40℃ is achieved. High strength and good low temperature performance.
Patent Information
- Application Number
- CN202310589779.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The existing marine cast steel materials are insufficient in low temperature toughness at -40℃, which cannot meet the requirements for the use conditions after the depth of the marine development area increases.
By controlling the types and content of elements, combining secondary normalization and primary tempering processes, microscopic segregation and crystal mixing phenomena are improved, low-temperature and high-strength toughness marine cast steel is prepared, with compositions including C, Si, Mn, Cr, Ni, Mo, Cu, etc. , V, P, S and other elements form ferrite, pearlite, and a small amount of bainite and nanoscale Cu precipitates.
The structural uniformity and low-temperature toughness of cast steel parts are improved, and the impact work is high and good, and the impact force reaches ≥130J in -40℃, the yield strength is ≥410MPa, the tensile strength is ≥530MPa, and the non-proportional elongation is ≥400MPa. Elongation rate ≥29%.
Smart Images

Figure CN119020678A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of marine cast steel materials, and in particular to a low-temperature high-strength and toughness marine cast steel and a preparation method thereof. Background Art
[0002] With the increasing number of marine development areas and depths in my country and the development of marine industry, the demand for marine cast steel materials is also increasing. The demand and development of marine cast steel is a new growth point for the future steel industry. Its harsh service environment determines that it must have excellent performance, such as high strength, high corrosion resistance, and good low-temperature toughness. At present, marine steel is gradually used in the Arctic Ocean with a temperature of -40 to -70℃, which puts higher requirements on the low-temperature toughness of marine cast steel materials. Therefore, how to improve low-temperature toughness has become one of the main problems in the manufacturing process of marine cast steel materials.
[0003] At present, there is no marine casting material that meets the requirements of -40℃ impact toughness KV2 of 50-200J in the relevant standards of commonly used marine cast steel materials. The existing commonly used cast steel materials have a V-mouth impact of 50J at -40℃. With the increasing marine development areas and depths, this low-temperature toughness gradually cannot meet the use conditions. Therefore, on the basis of ensuring that the strength meets the technical indicators, it is of great significance to prepare casting materials with -40℃ impact toughness KV2 of 50-200J and improve the application range of materials for the development of marine cast steel in my country. Summary of the invention
[0004] In view of the above situation, the present invention aims to provide a low-temperature high-strength and high-toughness marine cast steel and a preparation method thereof, so as to solve the problems of poor structural uniformity and low low-temperature toughness of existing marine cast steel materials.
[0005] The purpose of the present invention is mainly achieved through the following technical solutions:
[0006] The invention provides a low-temperature high-strength and toughness marine cast steel. The components of the low-temperature high-strength and toughness marine cast steel include, by mass percentage, C: 0.05%-0.11%, Si: 0.20%-0.40%, Mn: 0.70%-1.15%, Cr: 0.20%-0.40%, Ni: 1.6%-2.2%, Mo: 0.01%-0.05%, Cu: 0.8%-1.3%, V: ≤0.01%, P: ≤0.02%, S: ≤0.01%, and the balance is Fe and inevitable trace impurities.
[0007] Furthermore, the components of the low-temperature high-strength and toughness cast steel include, by mass percentage: C: 0.082%~0.092%, Si: 0.22%~0.30%, Mn: 1.0%~1.1%, Cr: 0.25%~0.35%, Ni: 1.8%~2.1%, Mo: 0.023%~0.024%, Cu: 0.8%~1.3%, V: ≤0.01%, P: ≤0.02%, S: ≤0.01%, and the balance is Fe and inevitable trace impurities.
[0008] The present invention also provides a method for preparing low-temperature high-strength and toughness marine cast steel, which is used to prepare the above-mentioned low-temperature high-strength and toughness marine cast steel, comprising the following steps:
[0009] Step 1: smelting and pouring to obtain steel castings;
[0010] Step 2: Primary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 1020-1070℃ and keep it warm, then cool it to below 200℃;
[0011] Step 3: Secondary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 850-950℃ and keep it warm, and then air cool it to below 100℃;
[0012] Step 4: High temperature tempering: Heat the steel casting to 550-640°C, keep warm, furnace cool or air cool to below 200°C to obtain low temperature high strength and toughness marine cast steel.
[0013] Furthermore, in step 2, during the process of heating the steel casting to 600-700°C for insulation, the heating rate is ≤50°C.
[0014] Furthermore, in step 2, the steel casting is heated to 600-700° C. and kept warm, and the holding time is calculated as 1h / 100mm, wherein 100mm is the thickness of the steel casting.
[0015] Furthermore, during the heating to 1020-1070°C insulation process, the heating rate is ≤70°C, and the insulation time is calculated as 1-3h / 100mm, where 100mm is the thickness of the steel casting.
[0016] Furthermore, in step 2, the furnace cooling rate is 20-150° C. / h.
[0017] Furthermore, in step 3, during the process of heating the steel casting to 600-700°C for insulation, the heating rate is ≤50°C, and the insulation time is calculated as 1h / 100mm, wherein 100mm is the thickness of the steel casting.
[0018] Furthermore, in step 3, the air cooling rate is ≥50°C / h.
[0019] Furthermore, the insulation time is calculated as 2 to 4 h / 100 mm, wherein 100 mm is the thickness of the steel casting.
[0020] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0021] 1. The size and wall thickness of marine castings are relatively large, and segregation is difficult to avoid in the cast state. Conventional preparation methods will cause mixed crystal phenomenon. The present invention controls the element types and element contents, especially the element contents of C and Mo elements, combines secondary normalizing and primary tempering processes, and diffuses the micro-segregated elements such as Cu, Ni, and C uniformly, effectively improving the micro-segregation and mixed crystal phenomenon. The grain size is 7-8, and the uniformity of the structure of the steel casting is improved.
[0022] 2. The present invention eliminates grain boundary carbides by controlling the type and content of elements and combining secondary normalizing and primary tempering processes, thereby effectively improving the impact toughness of steel castings. The steel castings prepared by the method of the present invention have a yield strength of ≥410Mpa, a tensile strength of ≥530MPa, an elongation strength of ≥400MPa when the non-proportional elongation is 0.2%, an elongation of ≥29%, a cross-sectional shrinkage of ≥61%, and an impact energy of ≥130J at -40°C. They have high mechanical strength and good low-temperature toughness.
[0023] 3. The present invention controls the type and content of elements and combines secondary normalizing and primary tempering to prepare a low-temperature, high-strength and tough marine cast steel. Unlike conventional methods that produce a large amount of bainite due to structural segregation, the marine cast steel of the present invention has a microstructure of ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates, a grain size of 7-8, a uniform structure, and good low-temperature toughness.
[0024] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0026] Figure 1a The metallographic structure diagram of the steel of Example 1 of the present invention is 100 times larger;
[0027] Figure 1b This is a 500-fold metallographic structure diagram of the steel of Example 1 of the present invention;
[0028] Figure 2a 100 times the metallographic structure diagram of the steel of Example 2 of the present invention;
[0029] Figure 2b This is a 500-fold metallographic structure diagram of the steel of Example 2 of the present invention;
[0030] Figure 3a The metallographic structure diagram is 100 times larger than that of the steel of Comparative Example 1 of the present invention;
[0031] Figure 3b The metallographic structure diagram is 500 times that of the steel of Comparative Example 1 of the present invention;
[0032] Figure 4a The metallographic structure diagram is 100 times larger than that of the steel of Comparative Example 2 of the present invention;
[0033] Figure 4b The metallographic structure diagram is 500 times that of the steel of Comparative Example 2 of the present invention;
[0034] Figure 5a is a scanning electron microscope image of the steel of Example 1 of the present invention;
[0035] Figure 5b This is a scanning electron microscope image of the steel of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0036] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used to illustrate the principles of the present invention together with the embodiments of the present invention.
[0037] The invention provides a low-temperature high-strength and toughness marine cast steel. The components of the low-temperature high-strength and toughness marine cast steel include, by mass percentage, C: 0.05%-0.11%, Si: 0.20%-0.40%, Mn: 0.70%-1.15%, Cr: 0.20%-0.40%, Ni: 1.6%-2.2%, Mo: 0.01%-0.05%, Cu: 0.8%-1.3%, V: ≤0.01%, P: ≤0.02%, S: ≤0.01%, and the balance is Fe and inevitable trace impurities.
[0038] The present invention uses a carbon equivalent range to accurately control the components of low-temperature high-strength and tough cast steel, the carbon equivalent is 0.50% to 0.58%, and at the same time satisfies 100C+Mn=9 to 10.5. The present invention controls the carbon equivalent and the chemical composition design approximate formula within the designed composition range.
[0039] The V-mouth impact energy of existing commonly used cast steel materials at -40°C is 50J. With the increasing marine development areas and depths, this low-temperature toughness gradually cannot meet the use conditions. The existing preparation method is used to prepare marine cast steel parts. Microsegregation and mixed crystal phenomena are easily generated during the heat treatment process, resulting in uneven organization and poor low-temperature toughness of cast steel parts. The present invention controls the element types and element contents, combines secondary normalizing and primary tempering processes, diffuses the microsegregated elements such as Cu, Ni, and C uniformly, effectively improves the microsegregation and mixed crystal phenomena, and the grain size is 7-8, which improves the organizational uniformity of the cast steel parts, has high mechanical strength and good low-temperature toughness.
[0040] The following is a detailed description of the effects and dosage of the components in the present invention:
[0041] C: Carbon is the most important element that determines the mechanical properties of steel. As the carbon content increases, the strength of the steel increases, while the plasticity and toughness decrease. Therefore, in order to ensure that the low-temperature high-strength and toughness marine cast steel of the present invention has a good low-temperature strength and toughness match, the C content in the present invention is controlled at 0.05% to 0.11%.
[0042] Si: Silicon can be dissolved in ferrite and austenite to increase the strength and hardness of steel, and can improve the tempering stability and oxidation resistance of steel, but too much silicon content will reduce the impact toughness and weldability of steel. Therefore, the content of Si in the present invention is controlled at 0.20% to 0.40%.
[0043] Mn: Mn is an essential element to ensure the strength and toughness of steel. Adding Mn can compensate for the strength loss caused by the reduction of C content. If the Mn content is too high, the hardenability of the steel will be increased, more martensitic structure will be formed, and the low-temperature toughness will be reduced. In order to comprehensively improve the strength and toughness, the Mn content in the present invention is in the range of 0.70% to 1.15%.
[0044] Cr: Chromium can increase the hardenability of steel and has a secondary hardening effect, which can improve the strength of carbon steel. Chromium can form a continuous solid solution with iron, reduce the austenite phase area, and add a certain amount of Cr to allow Cr, Mn, Ni, and Mo to work together to control the hardenability of the alloy and ensure the organizational ratio. Therefore, the content of Cr in the present invention is controlled at 0.20% to 0.40%.
[0045] Ni: Ni is a solid solution strengthening element that can strengthen ferrite and refine pearlite in steel. For low carbon steel, adding a certain amount of Ni can improve the strength and toughness of the steel, especially the low temperature toughness, but too much Ni will reduce the low temperature toughness and increase the cost. Therefore, the Ni content of the present invention is controlled at 1.6% to 2.2%.
[0046] Mo: Mo has the effect of solid solution strengthening in steel, improving hardenability, preventing temper brittleness, improving toughness, and expanding the γ phase region, playing an important role in controlling phase transformation structure, and can effectively improve material strength. However, as the Mo content increases, the yield strength of the steel increases, and too high a Mo content will damage the plasticity of the steel. Therefore, the Mo content of the present invention is controlled at 0.01% to 0.05%.
[0047] Cu: copper added to steel can not only effectively improve the strength and impact toughness of steel, but also enhance its corrosion resistance and improve the quality of steel castings. The copper content in steel is greater than 0.8%. Through solid solution and aging treatment, precipitation strengthening effect can be achieved to increase strength, but when the content exceeds 1.3%, the steel will become brittle. Therefore, in order to ensure that the copper-containing cast steel material has high strength and good low-temperature toughness, the content of Cu in the present invention is controlled at 0.8% to 1.3%.
[0048] V: V element can refine the structure and grain of steel, improve the strength and yield ratio after normalizing and low temperature characteristics, improve welding performance, and for thick wall casting materials, V needs to be added to refine the grains and ensure the grain size level. Therefore, the content of V in the present invention is controlled to be ≤0.01%.
[0049] P: P element is an impurity in steel, which is not conducive to weldability and toughness. Therefore, in the present invention, the P content is controlled to be ≤0.02%.
[0050] S: S element is an impurity in steel, which seriously deteriorates the corrosion resistance and toughness of steel. Therefore, in the present invention, the S content is controlled to be ≤0.01%.
[0051] Preferably, a low-temperature high-strength and toughness marine cast steel is provided, wherein the components of the low-temperature high-strength and toughness marine cast steel include, by mass percentage: C: 0.082% to 0.092%, Si: 0.22% to 0.30%, Mn: 1.0% to 1.1%, Cr: 0.25% to 0.35%, Ni: 1.8% to 2.1%, Mo: 0.023% to 0.024%, Cu: 0.8% to 1.3%, V: ≤0.01%, P: ≤0.02%, S: ≤0.01%, and the remainder is Fe and inevitable trace impurities.
[0052] The present invention also provides a method for preparing low-temperature high-strength and toughness marine cast steel, which is used to prepare the above-mentioned low-temperature high-strength and toughness marine cast steel, comprising the following steps:
[0053] Step 1: smelting and pouring to obtain steel castings;
[0054] Step 2: Primary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 1020-1070℃ and keep it warm, then cool it to below 200℃;
[0055] Step 3: Secondary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 850-950℃ and keep it warm, and then air cool it to below 100℃;
[0056] Step 4: High temperature tempering: Heat the steel casting to 550-640°C, keep warm, furnace cool or air cool to below 200°C to obtain low temperature high strength and toughness marine cast steel.
[0057] Specifically, in step 2, the steel casting is first heated to 600-700°C for insulation, the insulation time is calculated as 1h / 100mm, and the heating rate is ≤50°C; this temperature range is the elastic-plastic transition temperature zone of the steel casting, and insulation within this temperature range is conducive to reducing the deformation of the steel casting caused by the temperature difference in different parts of the steel casting during the heating process due to the different wall thickness of the steel casting; the heating rate in this low temperature section is ≤50°C, and too fast heating temperature can easily lead to large temperature differences at different positions of the steel casting, thereby superimposing stress and causing deformation. After heat preservation, the temperature is continuously raised to 1020-1070°C, and high-temperature diffusion is performed within this temperature range. Elements such as Cu, Ni, and C that are prone to microscopic segregation will diffuse evenly, thereby avoiding the occurrence of mixed crystals and bainite segregation zones in the subsequent heat treatment process, and improving the uniformity of the organization. At the same time, since the carbides at the grain boundaries have a splitting effect on the matrix, the impact toughness of the material will be reduced. During the high-temperature heating process at 1020-1070°C, the carbides at the grain boundaries can be dissolved to improve the impact toughness of the steel casting. The heating rate in the low-temperature section is ≤70°C, because after 700°C, the steel casting has entered the plastic deformation zone, and the heating rate can be appropriately increased to improve efficiency and reduce energy consumption.
[0058] Specifically, since the grain size of the as-cast structure is relatively coarse, the grains of the as-cast structure are still relatively coarse after the first normalizing. Therefore, in step 3, the steel casting is subjected to secondary normalizing to refine the grains. First, the steel casting is heated to 600-700°C for insulation. The insulation time is calculated as 1h / 100mm and the heating rate is ≤50°C. A secondary normalizing of 850-950°C is added. After insulation at 600-700°C, the temperature is further increased to 850-950°C, the heating rate is ≤70°C, and the insulation time is calculated as 1-3h / 100mm. Then, it is cooled to below 100°C at a cooling rate of ≥50°C / h. After the secondary normalizing treatment, the grain size of the steel casting is significantly refined and can reach level 6.5-7.
[0059] Specifically, in step 4, the steel casting is heated to 550-640°C, the holding time is calculated as 2-4h / 100mm, the heating rate is ≤50°C, and then furnace cooling or air cooling to below 200°C is performed to obtain low-temperature, high-strength and tough marine cast steel; the tempering treatment can improve the structure of the steel casting, transform the normalized structure into the tempered structure, and at the same time, the Cu element dissolved in the matrix is precipitated to form small nano-scale point precipitates, which play a precipitation strengthening role and can effectively improve the toughness of the steel casting; in addition, the tempering process eliminates the thermal stress and organizational stress generated during the normalizing process of the steel casting, and stabilizes the product size.
[0060] The low-temperature high-strength and tough marine cast steel prepared by the method of the present invention has a microstructure of ferrite+pearlite+a small amount of bainite+nano-level Cu precipitates, and a grain size of 7.5-8.
[0061] The hull structural steel prepared by the present invention has a yield strength of ≥410 MPa (such as 411-420 MPa), a tensile strength of ≥530 MPa (such as 540-543 MPa), an elongation strength of ≥400 MPa (such as 406-417 MPa) when the non-proportional elongation is 0.2%, an elongation of ≥29% (such as 29-31.5%), a cross-sectional shrinkage of ≥61% (such as 61-75%), an impact energy of ≥130 J (such as 139-265 J) at -40°C, and has good low-temperature toughness.
[0062] The advantages of the precise control of the chemical composition, content and preparation process parameters of the present invention will be demonstrated below with specific examples and comparative examples.
[0063] Example 1
[0064] A low-temperature high-strength and tough marine cast steel, the components of which are, by mass percentage, C: 0.082%, Si: 0.30%, Mn: 1.1%, Cr: 0.35%, Ni: 2.1%, Mo: 0.024%, Cu: 1.05%, V: 0.01%, P: 0.02%, S: 0.01%, the remainder being Fe and inevitable trace impurities; the carbon equivalent is 0.55%. The preparation method thereof comprises the following steps:
[0065] Step 1: Smelting and pouring to obtain a steel casting: the thickness of the steel casting is 500 mm;
[0066] Step 2: Primary normalizing: Heat the steel casting to 650℃ at a heating rate of 50℃ / h and keep it warm for 5h, then continue to heat it to 1050℃ at a heating rate of 70℃ / h, heat it for 10h, then cool it to below 200℃ at a cooling rate of 30-80℃ / h;
[0067] Step 3: Secondary normalizing: heat the steel casting to 650℃ at a heating rate of 50℃ / h, keep it at that temperature for 5h, then continue to heat it to 920℃ at a heating rate of 70℃ / h, keep it at that temperature for 10h, and then air cool it to below 100℃ at a cooling rate of 80-150℃ / h;
[0068] Step 4: High temperature tempering: Heat the steel casting to 590°C at a heating rate of 50°C / h, heat and keep warm for 15 hours, and air cool to below 200°C to obtain low-temperature high-strength and tough cast steel.
[0069] The microstructure of the low-temperature high-strength and toughness marine cast steel prepared in this embodiment is ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates; the grain size is 7.5-8.
[0070] The mechanical properties are: yield strength is 421MPa; tensile strength is 543MPa; extension strength is 417MPa when the non-proportional elongation is 0.2%, elongation is 31.5%, cross-sectional shrinkage is 75%, and the minimum impact energy at -40℃ is 141J.
[0071] Example 2
[0072] A low-temperature high-strength and tough marine cast steel, the components of which are, by mass percentage, C: 0.092%, Si: 0.22%, Mn: 1.0%, Cr: 0.25%, Ni: 1.8%, Mo: 0.023%, Cu: 1.05%, V: 0.01%, P: 0.01%, S: 0.008%, the remainder being Fe and inevitable trace impurities; the carbon equivalent is 0.51%. The preparation method thereof comprises the following steps:
[0073] Step 1: Smelting and pouring to obtain a steel casting: the thickness of the steel casting is 300 mm;
[0074] Step 2: Primary normalizing: heat the steel casting to 670℃ at a heating rate of 50℃ / h and keep it warm for 3h, then continue to heat it to 1020℃ at a heating rate of 70℃ / h, heat it for 6h, and then cool it to below 200℃ at a cooling rate of 30-80℃ / h;
[0075] Step 3: Secondary normalizing: heat the steel casting to 670°C at a heating rate of 50°C / h, keep it at that temperature for 3 hours, then continue to heat it to 870°C at a heating rate of 70°C / h, keep it at that temperature for 6 hours, and then air cool it to below 100°C at a cooling rate of 80-150°C / h;
[0076] Step 4: High temperature tempering: Heat the steel casting to 600°C at a heating rate of 50°C / h, heat and keep warm for 9 hours, and air cool to below 200°C to obtain low-temperature high-strength and tough cast steel.
[0077] The microstructure of the low-temperature high-strength and toughness marine cast steel prepared in this embodiment is ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates; the grain size is 7.5-8.
[0078] The mechanical properties are: yield strength is 411MPa; tensile strength is 540MPa; extension strength is 406MPa when the non-proportional elongation is 0.2%, elongation is 29%, cross-sectional shrinkage is 61%, and the minimum impact energy at -40℃ is 206J.
[0079] Example 3
[0080] A low-temperature high-strength and tough marine cast steel, the components of which are, by mass percentage, C: 0.082%, Si: 0.30%, Mn: 1.1%, Cr: 0.35%, Ni: 2.1%, Mo: 0.024%, Cu: 1.05%, V: 0.01%, P: 0.02%, S: 0.01%, the remainder being Fe and inevitable trace impurities; the carbon equivalent is 0.55%. The preparation method thereof comprises the following steps:
[0081] Step 1: Smelting and pouring to obtain a steel casting: the thickness of the steel casting is 500 mm;
[0082] Step 2: Primary normalizing: heat the steel casting to 670℃ at a heating rate of 50℃ / h and keep it warm for 5h, then continue to heat it to 1020℃ at a heating rate of 70℃ / h, heat it for 10h, then cool it to below 200℃ at a cooling rate of 30-80℃ / h;
[0083] Step 3: Secondary normalizing: The heating rate is 50℃ / h, the steel casting is heated to 670℃, kept at this temperature for 5h, then continued to heat to 870℃ at a heating rate of 70℃ / h, kept at this temperature for 10h, and then air-cooled to below 100℃ at a cooling rate of 80-150℃ / h;
[0084] Step 4: High temperature tempering: Heat the steel casting to 600°C at a heating rate of 50°C / h, heat and keep warm for 15 hours, and air cool to below 200°C to obtain low-temperature high-strength and tough cast steel.
[0085] The microstructure of the low-temperature high-strength and toughness marine cast steel prepared in this embodiment is ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates; the grain size is 7.5-8.
[0086] The mechanical properties are: yield strength is 419MPa; tensile strength is 541MPa; elongation strength is 414MPa when the non-proportional elongation is 0.2%, elongation is 30%, cross-sectional shrinkage is 72%, and the minimum impact energy at -40℃ is 139J.
[0087] Comparative Example 1
[0088] A low-temperature high-strength and tough marine cast steel comprises, by mass percentage, 0.13% C, 0.29% Si, 1.13% Mn, 0.36% Cr, 2.01% Ni, 0.15% Mo, 1.06% Cu, 0.01% V, 0.02% P, 0.008% S, and the remainder is Fe and inevitable trace impurities; the carbon equivalent is 0.63%.
[0089] The preparation method and parameters are the same as those in Example 1.
[0090] In this comparative example, the Mo element and the C element are beyond the scope of the present invention. This comparative example has structural segregation, the segregation zone has chaotic structure, the microstructure is a mixture of granular bainite and upper bainite, and the grain size is 7-7.5.
[0091] The mechanical properties are as follows: yield strength is 457 MPa; tensile strength is 592 MPa; elongation strength is 453 MPa when the non-proportional elongation is 0.2%, elongation is 34%, cross-sectional shrinkage is 79%, the minimum impact energy at -40°C is 19 J and the maximum is 57 J, and the low-temperature toughness is much lower than that of Example 1.
[0092] Comparative Example 2
[0093] The components and proportions of the steel castings in this comparative example are the same as those in Example 1.
[0094] The preparation method of this comparative example comprises the following steps:
[0095] Step 1: Smelting and pouring to obtain a steel casting: the thickness of the steel casting is 500 mm.
[0096] Step 2: Normalizing: Heat the steel casting to 650°C at a heating rate of 50°C / h, keep it at that temperature for 5 hours, then continue to heat it to 920°C at a heating rate of 70°C / h, keep it at that temperature for 10 hours, and then air cool it to below 100°C at a cooling rate of 80°C / h;
[0097] Step 3: High temperature tempering: heat the steel casting to 590°C at a heating rate of 50°C / h, heat and keep warm for 15 hours, and air cool to below 200°C to obtain the steel casting.
[0098] This comparative example was normalized only once without high-temperature diffusion, and there was organizational segregation. The microstructure was ferrite + pearlite + more bainite, and the grain size was 6-7.5.
[0099] The mechanical properties are as follows: yield strength is 423 MPa; tensile strength is 536 MPa; elongation strength is 419 MPa when the non-proportional elongation is 0.2%, elongation is 30%, cross-sectional shrinkage is 73%, the minimum impact energy at -40°C is 21 J and the maximum is 57 J, and the low-temperature toughness is much lower than that of Example 1.
[0100] Table 1 Chemical composition of steel of embodiment and comparative example (%)
[0101] serial number C Si Mn P S Cr Ni Mo V Cu Example 1 0.082 0.3 1.1 0.02 0.01 0.35 2.1 0.024 0.01 1.05 Example 2 0.092 0.22 1.0 0.01 0.008 0.25 1.8 0.023 0.01 1.05 Example 3 0.082 0.3 1.1 0.02 0.01 0.35 2.1 0.024 0.01 1.05 Comparative Example 1 0.13 0.29 1.13 0.02 0.008 0.36 2.01 0.15 0.01 1.06 Comparative Example 2 0.082 0.3 1.1 0.02 0.01 0.35 2.1 0.024 0.01 1.05
[0102] Table 2 Microstructure of steel of embodiment and comparative example
[0103] Serial number Microstructure Grain size Example 1 Ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates Level 7.5-8 Example 2 Ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates Level 7.5-8 Example 3 Ferrite + pearlite + a small amount of bainite + nano-scale Cu precipitates Level 7.5-8 Comparative Example 1 Severe organizational segregation, a large amount of bainite + ferrite + pearlite + nano-scale Cu precipitates Level 7-7.5 Comparative Example 2 Severe organizational segregation, a large amount of bainite + ferrite + pearlite + nano-scale Cu precipitates Level 6-7.5
[0104] Table 3 Mechanical properties of steels of embodiments and comparative examples
[0105]
[0106] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A low temperature, high strength and toughness marine cast steel, It is characterized in that The components of low temperature high strength and toughness marine cast steel include, by mass percentage: C: 0.05% ~ 0.11%, Si: 0.20% ~ 0.40%, Mn: 0.70% ~ 1.15%, Cr: 0.20% ~ 0.40%, Ni: 1.6% ~ 2.2%, Mo: 0.01% ~ 0.05%, Cu: 0.8% ~ 1.3%, V: ≤ 0.01%, P: ≤ 0.02%, S: ≤ 0.01%, and the balance is Fe and inevitable trace impurities.
2. The low temperature high strength and toughness marine cast steel according to claim 1, It is characterized in that The components of the low-temperature high-strength and toughness cast steel include, by mass percentage: C: 0.082% to 0.092%, Si: 0.22% to 0.30%, Mn: 1.0% to 1.1%, Cr: 0.25% to 0.35%, Ni: 1.8% to 2.1%, Mo: 0.023% to 0.024%, Cu: 0.8% to 1.3%, V: ≤0.01%, P: ≤0.02%, S: ≤0.01%, and the remainder is Fe and inevitable trace impurities.
3. A method for preparing low-temperature high-strength and high-toughness marine cast steel, used for preparing the low-temperature high-strength and high-toughness marine cast steel according to claim 1 or 2, It is characterized in that The following steps are involved: Step 1: smelting and pouring to obtain steel castings; Step 2: Primary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 1020-1070℃ and keep it warm, then cool it to below 200℃; Step 3: Secondary normalizing: heat the steel casting to 600-700℃ and keep it warm, then continue to heat it to 850-950℃ and keep it warm, and then air cool it to below 100℃; Step 4: High temperature tempering: Heat the steel casting to 550-640°C, keep warm, furnace cool or air cool to below 200°C to obtain low temperature high strength and toughness marine cast steel.
4. The preparation method according to claim 3, It is characterized in that In step 2, during the heat preservation process of heating the steel casting to 600-700°C, the heating rate is ≤50°C.
5. The preparation method according to claim 4, It is characterized in that In step 2, the steel casting is heated to 600-700° C. and kept warm. The holding time is calculated as 1h / 100mm, where 100mm is the thickness of the steel casting.
6. The preparation method according to claim 5, It is characterized in that In step 2, during the temperature increase to 1020-1070° C. and insulation process, the heating rate is ≤70° C., and the insulation time is calculated as 1-3h / 100mm, where 100mm is the thickness of the steel casting.
7. The preparation method according to claim 6, It is characterized in that In step 2, the furnace cooling rate is 20-150° C. / h.
8. The preparation method according to claim 7, It is characterized in that In step 3, during the process of heating the steel casting to 600-700° C. and holding the temperature, the heating rate is ≤50° C., and the holding time is calculated as 1h / 100mm, where 100mm is the thickness of the steel casting.
9. The preparation method according to claim 8, It is characterized in that In step 3, the air cooling rate is ≥50°C / h.
10. The preparation method according to claim 9, It is characterized in that In step 4, the insulation time is calculated as 2 to 4 h / 100 mm, where 100 mm is the thickness of the steel casting.