Abrasion-resistant stainless steel amorphous composite coating material and preparation method thereof

By using liquid metal atomization, plasma spraying and cold spraying technology on aluminum alloy substrates, the problem of low abrasion resistance of existing coatings is solved and efficient wear resistance is achieved. and prolong service life.

CN119020781APending Publication Date: 2024-11-26LANZHOU UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411138246.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing aluminum matrix/stainless steel coating has low wear resistance, limiting its service life and performance in engineering applications such as light tank hubs and shells.

Method used

The stainless steel amorphous composite coating is prepared on the aluminum alloy substrate by liquid metal atomization, plasma spraying and cold spraying technology. By forming a raised, stainless steel-aluminum alloy composite crystal layer and stainless steel amorphous layer, and microcrystalization treatment is carried out. , improve the abrasion resistance of the coating.

Benefits of technology

It significantly improves the abrasion resistance of the coating, enhances the binding force between the coating and the substrate, reduces porosity and defects, extends service life, and maintains stability in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000003530000171
    Figure BDA0005000003530000171
Patent Text Reader

Abstract

The invention discloses a wear-resistant stainless steel amorphous composite coating material and a preparation method thereof, and relates to the technical field of stainless steel coating preparation.The preparation method comprises the steps that firstly, aluminum alloy serves as a base material, after surface treatment, a liquid metal atomization method is used for spraying the surface of the base material to form protrusions, and then the protrusions are hardened; the preparation method comprises the following steps: preparing a base material, spraying a stainless steel-aluminum alloy composite crystal layer on the to-be-sprayed surface of the base material by using a plasma spraying method, preparing a stainless steel amorphous layer on the surface of the composite crystal layer by using a cold spraying method, and finally carrying out micro-crystallization treatment on the stainless steel amorphous layer to finally obtain the stainless steel amorphous composite coating material. The method has the advantages of high component control precision, high process stability and repeatability and capability of realizing excellent abrasion resistance of the stainless steel coating material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel coating preparation, and in particular to a wear-resistant stainless steel amorphous composite coating material and a preparation method thereof. Background Art

[0002] The light metal ultra-thick stainless steel coating technology mainly deposits one or more layers of stainless steel materials on a light metal substrate (such as aluminum alloy) through a specific process method to increase the surface hardness, wear resistance, corrosion resistance and improve the appearance of the substrate. This coating technology can significantly improve the service life and performance of light metal products. When preparing ultra-thick stainless steel coatings on light metal substrates, multi-layer coating technology can be used to alternately deposit stainless steel and other materials (such as transition layers, reinforcement layers, etc.) to achieve the preparation of ultra-thick coatings.

[0003] With the continuous development of materials science and surface engineering technology, ultra-thick stainless steel coating technology will continue to be optimized and improved. Emerging technologies such as multi-layer coating technology and nanotechnology will be more widely used in the preparation of ultra-thick stainless steel coatings to improve the comprehensive performance of the coatings. Light metal ultra-thick stainless steel coating technology is a complex and important field involving a variety of process methods and technical challenges.

[0004] Light metal ultra-thick stainless steel coatings are mainly used in light tank wheels and shells. They must not only meet the requirements of wear resistance and corrosion resistance, but also have a certain thickness (generally, the coating thickness is positively correlated with the coating life). Under actual working conditions, the damage to the coating mainly comes from three aspects. First, due to the low bonding rate of the surface lamellar tissue and microcracks, its hardness is low and its wear resistance is poor, making it difficult to resist high-load friction conditions, resulting in rapid wear and failure of the coating; second, the unevenness and porosity of the overall lamellar tissue of the coating can easily lead to fatigue failure; third, the internal porosity of the coating, the lamellar tissue is not tightly bonded, and the gaps formed allow salt spray and seawater to pass through these defects to form a spatial network, making it difficult to resist Cl + Long-term corrosion causes a significant decrease in the corrosion resistance of the coating. Therefore, improving the wear resistance of the coating is an important factor in improving the service performance of the coating. Improving the wear resistance of the aluminum substrate / stainless steel coating through a series of methods such as liquid metal atomization, plasma spraying, cold spraying and microcrystallization heat treatment is a key means to solve the above engineering problems. Summary of the invention

[0005] The present invention aims at the problem that the existing aluminum substrate / stainless steel coating has low wear resistance and limits its engineering application, and provides a wear-resistant stainless steel amorphous composite coating material and a preparation method thereof.

[0006] In order to achieve the above object, the present invention is implemented by adopting the following technical scheme:

[0007] In a first aspect, the present invention provides a method for preparing a wear-resistant stainless steel amorphous composite coating material, comprising the following steps:

[0008] An aluminum alloy substrate is used as a substrate, and after surface treatment, a liquid metal atomization method is used to spray on the surface of the substrate to form protrusions, and then the protrusions are hardened to obtain an aluminum alloy substrate to be sprayed;

[0009] A stainless steel-aluminum alloy composite crystal layer is formed on the surface of the aluminum alloy substrate to be sprayed by a plasma spraying method, and then a stainless steel amorphous layer is prepared on the surface of the stainless steel-aluminum alloy composite crystal layer by a cold spraying method. The stainless steel amorphous layer is then microcrystallized to obtain a wear-resistant stainless steel amorphous composite coating material.

[0010] As a further improvement of the present invention, the grade of the aluminum alloy is 2017 or 2024.

[0011] As a further improvement of the present invention, the surface treatment is to remove burrs on the surface of the aluminum alloy substrate by magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness ≥ HB180, the magnetic brush rotates at a speed of 130 to 150 rpm, and the surface roughness of the substrate after grinding is ≤ Ra0.04 microns.

[0012] The magnetic grinding machine works in an automated way, reducing the need for manual operation, thus greatly improving the efficiency of burr removal. Because the magnetic abrasive can be evenly distributed on the surface of the aluminum alloy under the action of magnetic force, it can completely and efficiently remove the burrs on the surface to avoid omissions.

[0013] The surface roughness of the substrate after grinding can be controlled at ≤Ra0.04 microns, which is a very fine surface treatment effect, which helps to improve the overall quality of the product. Since the magnetic grinding machine uses magnetic force as the power source, the polishing effect is more consistent, ensuring the consistency of the product surface quality. The magnetic grinding method has good adaptability to aluminum alloy substrates of different shapes and sizes, and can meet the processing requirements of different products. Using iron-based powder with a surface hardness of ≥HB180 as an abrasive, while removing burrs, it may also increase the hardness of the substrate surface to a certain extent and enhance its wear resistance.

[0014] As a further improvement of the present invention, the liquid metal atomization method specifically includes:

[0015] The same grade of aluminum alloy as the substrate is used as the raw material, argon gas at 560-630°C is used as the power source, the ejection speed is 180-220 m / s, the metal droplets are air-cooled on the surface of the substrate, and finally protrusions are formed on the surface of the substrate with an arrangement density of 3200-3500 per square millimeter.

[0016] Using aluminum alloy of the same grade as the substrate as the raw material ensures that the chemical and physical properties between the coating and the substrate are highly consistent, which is conducive to enhancing the bonding between the coating and the substrate and improving the stability and durability of the overall structure. Using high-temperature argon gas at 560-630°C as the power source not only provides enough energy to spray metal droplets at high speed, but also helps the metal droplets to melt and spread quickly on the surface of the substrate to form a uniform and dense coating. The spraying speed reaches 180-220 m / s. This high-speed spraying technology can ensure that the metal droplets hit the surface of the substrate with extremely high kinetic energy, forming a strong metallurgical bond, while reducing pores and defects in the coating.

[0017] The metal droplets protruding on the surface of the substrate are arranged at a density of 3200 to 3500 per square millimeter. This high-density arrangement makes the coating have a more uniform and dense microstructure, thereby improving the hardness, wear resistance and corrosion resistance of the coating. The metal droplets solidify in air cooling on the surface of the substrate, which helps to form a fine grain structure and further improve the mechanical properties and fatigue resistance of the coating.

[0018] As a further improvement of the present invention, the hardening treatment of the protrusions comprises:

[0019] The substrate surface is convexly heated to 530-550°C and then water-cooled.

[0020] As a further improvement of the present invention, the method of using a plasma spraying method to spray a stainless steel-aluminum alloy composite crystal layer on the surface of the aluminum alloy substrate to be sprayed comprises:

[0021] Plasma spraying uses 130-150 micron 2017 or 2024 aluminum alloy powder and 110-130 micron stainless steel powder as raw materials, the mass percentage of aluminum alloy powder and stainless steel powder is (19-25): (75-81), the spraying distance is 32-38 mm, the argon gas flow rate is 47-55 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer is 110-140 microns.

[0022] Aluminum alloy powder has good light weight, high strength and corrosion resistance, while stainless steel powder is known for its excellent wear resistance, high temperature resistance and oxidation resistance. The combination of the two can make full use of their respective advantages to form a composite coating with comprehensive performance. By adjusting the mass percentage of aluminum alloy powder and stainless steel powder, the performance of the coating can be customized according to specific application requirements to meet the use requirements under different working conditions.

[0023] Precise control of spraying distance, argon flow rate and other parameters helps to ensure uniformity and density of the coating and reduce the generation of pores and defects. Reasonable spraying parameter settings can improve spraying efficiency, shorten production cycle and reduce production costs.

[0024] The formation of the stainless steel-aluminum alloy composite crystal layer makes the coating not only have the wear resistance, high temperature resistance, and oxidation resistance of stainless steel, but also have the light weight, high strength, and corrosion resistance of aluminum alloy, thus significantly improving the overall performance of the coating. The coating thickness is controlled between 110 and 140 microns, which can ensure that the coating has sufficient thickness to provide a lasting protective effect, while avoiding problems such as cracking or shedding of the coating caused by excessive thickness.

[0025] As a further improvement of the present invention, the method of preparing a stainless steel amorphous layer on the surface of the stainless steel-aluminum alloy composite crystal layer by cold spraying comprises:

[0026] Using the cold spraying method, 25-50 micron stainless steel amorphous powder is used as raw material, and a 110-130 micron thick amorphous layer is sprayed on the surface of the composite crystal layer at 20-28°C. The compressed gas is nitrogen and the speed is 500-700 m / s.

[0027] During the cold spraying process, stainless steel amorphous powder can form an amorphous coating on the substrate surface due to mechanisms such as high-speed impact and adiabatic shear instability. The amorphous structure has unique physical and chemical properties, such as high hardness, high strength, excellent corrosion resistance and wear resistance, which enable the coating to maintain long-term stability in harsh environments. The thickness of the amorphous layer is precisely controlled between 110 and 130 microns, which helps ensure that the coating has sufficient protection while avoiding problems such as cracking or shedding of the coating due to excessive thickness.

[0028] The stainless steel amorphous powder of 25 to 50 microns is selected as the spraying raw material. This particle size range helps the powder particles to undergo sufficient plastic deformation and effective deposition during high-speed impact, thereby improving the density and bonding strength of the coating. Spraying is carried out at room temperature of 20 to 28°C to avoid the adverse effects of high temperature on coating performance, while reducing energy consumption and production costs.

[0029] Nitrogen is used as compressed gas and sprayed at a high speed of 500-700 m / s. The high speed ensures that the powder particles can fully impact the surface of the substrate and undergo plastic deformation, thus forming a high-quality coating.

[0030] Cold spraying technology itself is a green spraying technology. No harmful substances or exhaust gas will be generated during the spraying process, and it does not pollute the environment. In addition, the powder splashed by spraying can be recycled and reused, further improving the utilization rate of materials. Cold spraying technology has the advantages of high spraying rate and high deposition efficiency. When preparing a stainless steel amorphous layer on the surface of a stainless steel-aluminum alloy composite crystal layer, a uniform and dense coating can be quickly formed, improving production efficiency.

[0031] The combination of stainless steel amorphous layer and stainless steel-aluminum alloy composite crystal layer further improves the comprehensive performance of the coating. The composite coating not only has the wear resistance and corrosion resistance of stainless steel, but also has the high hardness and high strength of amorphous materials, which can meet the use requirements under more complex working conditions.

[0032] As a further improvement of the present invention, the microcrystallization treatment of the stainless steel amorphous layer comprises:

[0033] The coating is crystallized by heat treatment, and is kept at 360-430°C for 45-63 minutes, and then air-cooled.

[0034] Microcrystallization can rearrange the atoms in the amorphous coating to form finer grains. These fine grains help improve the hardness and strength of the coating, making it more wear-resistant and scratch-resistant. Appropriate microcrystallization can improve the toughness of the coating to a certain extent and reduce cracking or peeling caused by excessive brittleness.

[0035] The surface of the coating after microcrystallization is more compact, with fewer pores and defects, thus improving the corrosion resistance of the coating, especially in humid and highly corrosive environments. The coating treated with microcrystallization can maintain good performance stability in high temperature environments and is not prone to softening, deformation or failure. The microcrystallization process helps to enhance the bonding between the coating and the substrate, improve the chemical stability of the coating, and reduce the coating shedding or performance degradation caused by chemical reactions.

[0036] In a second aspect, the present invention provides a wear-resistant stainless steel amorphous composite coating material, which is prepared by the preparation method of the wear-resistant stainless steel amorphous composite coating material.

[0037] As a further improvement of the present invention, the prepared stainless steel coating material has an amorphous composite structure, the coating and interface porosity is ≤0.7%, the coating / substrate interface bonding strength is ≥47MPa, the coating surface hardness is ≥420HV1, the sliding friction test wear amount is ≤1.4 micrograms per square centimeter per hour, and the 50g / L sodium chloride salt spray resistance test corrosion weight loss is ≤0.4 micrograms per square centimeter per hour.

[0038] Compared with the prior art, the present invention has the following characteristics and advantages:

[0039] The present invention first uses aluminum alloy as a substrate, sprays the substrate surface with a liquid metal atomization method after surface treatment to form protrusions, then hardens the protrusions, and then uses a plasma spraying method to spray a stainless steel-aluminum alloy composite crystal layer on the surface to be sprayed of the substrate, and then uses a cold spraying method to prepare a stainless steel amorphous layer on the surface of the composite crystal layer, and finally performs a microcrystallization treatment on the stainless steel amorphous layer; wherein the aluminum alloy protrusions are prepared on the substrate surface by using a liquid metal atomization method, the purpose is to increase the metallurgical bonding surface between the substrate and the coating and improve the interface bonding strength to ensure the safety and long life of the coating during service; the stainless steel-aluminum alloy composite crystal layer is used as a transition layer to balance the overall toughness and strength of the coating and the substrate; the stainless steel amorphous layer is prepared by a cold spraying method, which can ensure the stability of the amorphous structure on the one hand, and on the other hand, utilize the advantages of high hardness, isotropy and no interface defects of the amorphous structure to effectively improve the wear resistance and corrosion resistance of the stainless steel coating; the microcrystallization treatment is used for the crystallization of the amorphous layer, which can improve the toughness of the amorphous layer and prevent the brittle fracture failure of the stainless steel during service. DETAILED DESCRIPTION

[0040] In order to make the method problems, method solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0041] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0042] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple.

[0043] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0044] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0045] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass in the embodiment description of the present application can be μg, mg, g, kg and other mass units known in the chemical industry.

[0046] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of method features indicated. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0047] The present invention provides a method for preparing a wear-resistant stainless steel amorphous composite coating material, comprising the following steps:

[0048] 1) An aluminum alloy is used as a substrate, and after surface treatment, a liquid metal atomization method is used to spray a protrusion on the surface of the substrate, and then the protrusion is hardened to obtain an aluminum alloy substrate to be sprayed;

[0049] 2) A stainless steel-aluminum alloy composite crystal layer is sprayed on the surface of the substrate to be sprayed by a plasma spraying method, and then a stainless steel amorphous layer is prepared on the surface of the composite crystal layer by a cold spraying method. Finally, the stainless steel amorphous layer is microcrystallized to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0050] The method for preparing the wear-resistant stainless steel amorphous composite coating material of the present invention realizes the preparation of a stainless steel amorphous composite coating with excellent wear resistance on an aluminum alloy substrate through a series of fine process steps. Each step is analyzed in detail as follows:

[0051] The pretreatment and convexity formation of aluminum alloy substrates specifically include:

[0052] Substrate selection: Aluminum alloy is chosen as the substrate because it has light weight, good processing performance and certain mechanical strength, making it an ideal choice for many industrial applications.

[0053] Surface treatment: Surface treatment of the substrate is an important step in coating preparation. It aims to remove oil, oxides and other impurities on the surface of the substrate, increase the surface roughness of the substrate, and thus enhance the bonding force between the coating and the substrate.

[0054] Liquid metal atomization and convexity formation: Liquid metal atomization is used to spray on the substrate surface to form convexities. This process not only increases the roughness of the substrate surface, but also provides more mechanical bite points for the subsequent coating adhesion. The convex structure can also disperse the stress concentration of the coating during use to a certain extent, improving the durability of the coating.

[0055] Bump hardening: Hardening the bumps can further increase their hardness and wear resistance, providing better support for subsequent coatings.

[0056] The preparation process of the composite crystal layer specifically includes:

[0057] Plasma spraying method: Use plasma spraying technology to spray stainless steel-aluminum alloy composite crystal layer on the surface to be sprayed of the substrate. Plasma spraying has the characteristics of high temperature, high speed and high energy density, which can ensure that the coating material is fully melted and quickly solidified during the spraying process to form a dense composite crystal layer. This layer not only has the corrosion resistance and wear resistance of stainless steel, but also improves the toughness and bonding strength of the coating through the addition of aluminum alloy.

[0058] The preparation and microcrystallization treatment of stainless steel amorphous layer specifically includes:

[0059] Cold spraying method: The stainless steel amorphous layer is prepared by cold spraying on the surface of the composite crystal layer. Cold spraying technology accelerates the powder particles to supersonic speed through high-speed airflow, and then hits the surface of the substrate, so that the powder particles undergo plastic deformation in a very short time and deposit on the substrate to form an amorphous coating. This method avoids the influence of high temperature on the coating material and retains the high hardness and high wear resistance of the amorphous structure.

[0060] Microcrystallization treatment: Microcrystallization treatment of the amorphous layer of stainless steel can further improve the performance of the coating. Microcrystallization treatment uses appropriate heat treatment processes to crystallize some areas in the amorphous coating to form a microcrystalline structure. This microcrystalline structure can maintain the high hardness of the amorphous coating while also improving the toughness and corrosion resistance of the coating.

[0061] The wear-resistant stainless steel amorphous composite coating material of the present invention achieves comprehensive improvement in hardness, wear resistance, corrosion resistance and bonding strength of the coating through multiple steps such as pretreatment of the aluminum alloy substrate, liquid metal atomization to form protrusions, plasma spraying to prepare the composite crystal layer, cold spraying to prepare the stainless steel amorphous layer and microcrystallization treatment. Among them, the application of liquid metal atomization and cold spraying technology ensures that the coating can maintain its excellent amorphous structure during the preparation process; and the addition of the composite crystal layer further improves the comprehensive performance of the coating.

[0062] Among them, each step specifically includes the following steps:

[0063] 1) Using 2017 or 2024 grade aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness ≥ HB180, the magnetic brush rotates at a speed of 130 to 150 rpm, and the surface roughness of the substrate after grinding is ≤ Ra0.04 microns, and then using the same grade aluminum alloy as the substrate as a raw material, using a liquid metal atomization method to spray on the surface of the substrate to form protrusions, using 560 to 630° C. argon gas as a power source, the spraying speed is 180 to 220 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3200 to 3500 per square millimeter, and then using an induction heating device to heat the protrusions on the surface of the substrate to 530 to 550° C., and then water-cooling to obtain an aluminum alloy substrate to be sprayed;

[0064] Step 1: Magnetic grinding to remove burrs on the surface of aluminum alloy substrate;

[0065] Magnetic grinding method: Use the power of the magnetic field to drive the magnetic needle (or magnetic particles) with grinding media to rotate and roll at high speed on the surface of the workpiece. Through physical friction and chemical action, the burrs, oxide scale, stains and tiny unevenness on the surface of the aluminum alloy substrate are effectively removed to achieve the effect of polishing and leveling.

[0066] Magnetic abrasive: Use iron-based powder with surface hardness ≥ HB180 as magnetic abrasive to ensure sufficient hardness and wear resistance to effectively remove burrs on the surface of aluminum alloy.

[0067] Rotation speed: The rotation speed of the magnetic brush is controlled at 130-150 rpm. This speed range can ensure the grinding effect while avoiding excessive damage to the substrate.

[0068] Surface roughness: The surface roughness of the substrate after grinding is ≤Ra0.04 microns, meeting the high-precision surface finish requirements.

[0069] Step 2: Liquid metal atomization spraying to form bulges;

[0070] Liquid metal atomization: The aluminum alloy is heated to liquid state and atomized into fine droplets by an atomizing device. These droplets are sprayed onto the substrate surface at a speed of 180 to 220 m / s under the action of high-speed airflow (such as argon).

[0071] Air cooling solidification: The metal droplets are air cooled and solidified on the surface of the substrate to form a raised metal layer. This process utilizes the rapid cooling effect of the metal droplets during high-speed spraying to achieve rapid solidification of the metal.

[0072] Arrangement density: By controlling the spraying parameters (such as spraying speed, spraying angle, etc.), the aluminum alloy protrusions are arranged on the substrate surface at a density of 3200 to 3500 per square millimeter to ensure the uniformity and density of the coating.

[0073] Step 3: The induction heating device heats the protrusion;

[0074] Induction heating: Using the principle of electromagnetic induction, under the action of the alternating magnetic field, the protrusions on the surface of the substrate generate induced current and heat. By controlling the heating time and temperature (530-550°C), the protrusions can achieve the desired heat treatment effect.

[0075] Water cooling: After heating is completed, water cooling is used to quickly cool the protrusions to fix their organizational structure and properties.

[0076] 2) 130-150 μm 2017 or 2024 aluminum alloy powder and 110-130 μm stainless steel powder are selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder is 19-25:75-81, and a stainless steel-aluminum alloy composite crystal layer is sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance is 32-38 mm, the argon gas flow rate is 47-55 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer is 110-140 μm. Then, 25-50 μm stainless steel amorphous powder is used as a raw material, and a 110-130 μm amorphous layer is prepared on the surface of the composite crystal layer at 20-28° C. by a cold spraying method. The compressed gas is nitrogen, and the speed is 500-700 m / s. Finally, the stainless steel amorphous layer is subjected to microcrystallization treatment at 360-430° C. for 45-63 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0077] Step 4: plasma spraying stainless steel-aluminum alloy composite crystal layer;

[0078] Plasma spraying: Use high-temperature and high-speed plasma jet to heat powder materials (such as aluminum alloy and stainless steel powder) to a molten or semi-molten state, and spray them onto the surface of the substrate to form a coating. By controlling the spraying parameters (such as spraying distance, argon flow rate, etc.), the uniformity and quality of the coating are ensured.

[0079] Composite crystal layer: Aluminum alloy powder and stainless steel powder are mixed in a certain proportion and then sprayed to form a stainless steel-aluminum alloy composite crystal layer with excellent wear resistance.

[0080] Step 5: Prepare stainless steel amorphous layer by cold spraying;

[0081] Cold spraying: Based on supersonic gas jet technology, unmelted metal powder (such as stainless steel amorphous powder) is impacted onto the substrate surface at high speed and deposited on the substrate through plastic deformation to form a coating. In this process, the metal powder will not melt, thus retaining its original physical and chemical properties.

[0082] Amorphous layer: A stainless steel amorphous layer is prepared on the surface of the composite crystal layer by cold spraying technology to further improve the wear resistance of the coating. The amorphous structure has unique physical and chemical properties, such as high hardness and high wear resistance.

[0083] Step 6: Microcrystallization treatment;

[0084] Microcrystallization treatment: The amorphous layer of stainless steel is kept at 360430℃ (4563 minutes), and the amorphous layer undergoes microcrystallization transformation by controlling the heating temperature and holding time. This process helps to further improve the stability and wear resistance of the coating.

[0085] Air cooling: After the insulation is completed, air cooling is used to allow the coating to cool naturally to room temperature.

[0086] In summary, the entire process involves a variety of advanced technologies such as magnetic grinding, liquid metal atomization spraying, induction heating, plasma spraying, cold spraying and microcrystallization treatment. By precisely controlling the process parameters and conditions of each step, efficient and precise processing and modification of the surface of the aluminum alloy substrate can be achieved.

[0087] Furthermore, in the process of preparing stainless steel coating materials, the present invention aims at the problem that the wear resistance of existing aluminum substrate / stainless steel coatings is low, which limits their engineering applications. A series of methods such as liquid metal atomization, plasma spraying, cold spraying and microcrystallization heat treatment are used to study the relationship between substrate grade, surface treatment process parameters, metal atomization process parameters, plasma spraying process parameters, cold spraying process parameters, microcrystallization process parameters and the wear resistance of stainless steel coatings, that is, for stainless steel coating materials, the optimal substrate grade, surface treatment process parameters, metal atomization process parameters, plasma spraying process parameters, cold spraying process parameters and microcrystallization process parameters that maintain high wear resistance.

[0088] The prepared stainless steel coating material has an amorphous composite structure, the coating and interface porosity is ≤0.7%, the coating / substrate interface bonding strength is ≥47MPa, the coating surface hardness is ≥420HV1, the sliding friction test wear is ≤1.4 micrograms per square centimeter per hour, and the 50g / L sodium chloride salt spray test corrosion weight loss is ≤0.4 micrograms per square centimeter per hour.

[0089] This method has high composition control accuracy, strong process stability and repeatability, and can achieve excellent wear resistance of stainless steel coating materials.

[0090] The properties of the stainless steel coating materials prepared in the following examples are shown in Table 1.

[0091] Example 1

[0092] 1) Using 2017 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB205, the magnetic brush rotates at a speed of 130 rpm, and the surface roughness of the substrate after grinding is Ra0.04 microns, and then using 2017 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 560°C argon as a power source, the spraying speed is 180 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3200 per square millimeter, and then the protrusions on the surface of the substrate are heated to 530°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0093] 2) 130 micron 2017 aluminum alloy powder and 110 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 19:81, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 32 mm, the argon gas flow rate was 47 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 110 microns. Then, 25 micron stainless steel amorphous powder was used as the raw material, and a 110 micron amorphous layer was prepared on the surface of the composite crystal layer at 20°C by a cold spraying method. The compressed gas was nitrogen, and the speed was 500 m / s. Finally, the stainless steel amorphous layer was subjected to a microcrystallization treatment at 360°C for 45 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0094] Example 2

[0095] 1) Using 2024 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB210, the magnetic brush rotates at a speed of 150 rpm, and the surface roughness of the substrate after grinding is Ra0.03 microns, and then using 2024 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 630°C argon as a power source, the spraying speed is 220 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3500 per square millimeter, and then the protrusions on the surface of the substrate are heated to 540°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0096] 2) 150 micron 2024 aluminum alloy powder and 130 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 25:75, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 38 mm, the argon gas flow rate was 55 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 140 microns. Then, 50 micron stainless steel amorphous powder was used as the raw material, and a 130 micron amorphous layer was prepared on the surface of the composite crystal layer by a cold spraying method at 28°C. The compressed gas was nitrogen, and the speed was 700 m / s. Finally, the stainless steel amorphous layer was subjected to a microcrystallization treatment by keeping it at 430°C for 63 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0097] Example 3

[0098] 1) Using 2017 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB180, the magnetic brush rotates at a speed of 140 rpm, and the surface roughness of the substrate after grinding is Ra0.04 microns, and then using 2017 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 580°C argon as a power source, the spraying speed is 200 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3300 per square millimeter, and then the protrusions on the surface of the substrate are heated to 540°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0099] 2) 140 micron 2017 aluminum alloy powder and 120 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 21:79, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 34 mm, the argon gas flow rate was 49 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 120 microns. Then, 30 micron stainless steel amorphous powder was used as raw material, and a 120 micron amorphous layer was prepared on the surface of the composite crystal layer at 23°C by a cold spraying method. The compressed gas was nitrogen, and the speed was 600 m / s. Finally, the stainless steel amorphous layer was subjected to microcrystallization treatment at 430°C for 45 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0100] Example 4

[0101] 1) Using 2024 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB220, the magnetic brush rotates at a speed of 130 rpm, and the surface roughness of the substrate after grinding is Ra0.03 microns, and then using 2024 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 590°C argon as a power source, the spraying speed is 220 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3400 per square millimeter, and then the protrusions on the surface of the substrate are heated to 540°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0102] 2) 140 micron 2024 aluminum alloy powder and 130 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 23:77, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 36 mm, the argon gas flow rate was 55 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 140 microns. Then, 50 micron stainless steel amorphous powder was used as the raw material, and a 130 micron amorphous layer was prepared on the surface of the composite crystal layer by a cold spraying method at 28°C. The compressed gas was nitrogen, and the speed was 500 m / s. Finally, the stainless steel amorphous layer was subjected to a microcrystallization treatment by keeping it at 360°C for 45 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0103] The performance parameters of the stainless steel coating materials prepared in Examples 1 to 4 are shown in Table 1:

[0104] Table 1

[0105]

[0106] It can be concluded from the above table that the prepared stainless steel coating material has an amorphous composite structure, the coating and interface porosity ≤0.7%, the coating / substrate interface bonding strength ≥47MPa, the coating surface hardness ≥420HV1, the sliding friction test wear ≤1.4 micrograms per square centimeter per hour, and the 50g / L sodium chloride salt spray test corrosion weight loss ≤0.4 micrograms per square centimeter per hour.

[0107] Example 5

[0108] 1) Using 2024 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB210, the magnetic brush rotates at a speed of 135 rpm, and the surface roughness of the substrate after grinding is Ra0.035 microns, and then using 2024 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 600°C argon as a power source, the spraying speed is 210 meters per second, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3300 per square millimeter, and then the protrusions on the surface of the substrate are heated to 540°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0109] 2) 145 micron 2024 aluminum alloy powder and 120 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 20:80, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 37 mm, the argon gas flow rate was 50 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 135 microns. Then, 45 micron stainless steel amorphous powder was used as the raw material, and a 125 micron amorphous layer was prepared on the surface of the composite crystal layer by a cold spraying method at 27°C. The compressed gas was nitrogen, and the speed was 680 meters per second. Finally, the stainless steel amorphous layer was subjected to a microcrystallization treatment at 420°C for 62 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0110] Example 6

[0111] 1) Using 2017 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB180, the magnetic brush rotates at a speed of 141 rpm, and the surface roughness of the substrate after grinding is Ra0.02 microns, and then using 2017 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 620°C argon as a power source, the spraying speed is 190 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3450 per square millimeter, and then the protrusions on the surface of the substrate are heated to 535°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0112] 2) 135 micron 2017 aluminum alloy powder and 125 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 22:78, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 37 mm, the argon gas flow rate was 48 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 124 microns. Then, 34 micron stainless steel amorphous powder was used as raw material, and a 115 micron amorphous layer was prepared on the surface of the composite crystal layer at 26°C by a cold spraying method. The compressed gas was nitrogen, and the speed was 550 m / s. Finally, the stainless steel amorphous layer was subjected to microcrystallization treatment at 420°C for 48 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0113] Example 7

[0114] 1) Using 2024 aluminum alloy as a substrate, removing burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of HB220, the magnetic brush rotates at a speed of 130 rpm, and the surface roughness of the substrate after grinding is Ra0.03 microns, and then using 2024 aluminum alloy as a raw material, spraying on the surface of the substrate to form protrusions by a liquid metal atomization method, using 590°C argon as a power source, the spraying speed is 220 m / s, the metal droplets are air-cooled on the surface of the substrate, and the arrangement density of the aluminum alloy protrusions on the surface of the substrate is 3400 per square millimeter, and then the protrusions on the surface of the substrate are heated to 540°C by an induction heating device, and then water-cooled to obtain an aluminum alloy substrate to be sprayed;

[0115] 2) 132 micron 2024 aluminum alloy powder and 115 micron stainless steel powder were selected as raw materials, the mass percentage of plasma sprayed aluminum alloy powder and stainless steel powder was 21:79, and a stainless steel-aluminum alloy composite crystal layer was sprayed on the surface to be sprayed of the substrate by a plasma spraying method. The spraying distance was 34 mm, the argon gas flow rate was 49 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer was 118 microns. Then, 35 micron stainless steel amorphous powder was used as the raw material, and a 119 micron amorphous layer was prepared on the surface of the composite crystal layer by a cold spraying method at 23°C. The compressed gas was nitrogen, and the speed was 560 m / s. Finally, the stainless steel amorphous layer was subjected to a microcrystallization treatment at 410°C for 48 minutes, and air-cooled to finally obtain a wear-resistant stainless steel amorphous composite coating material.

[0116] The stainless steel coating material prepared in Examples 5-7 has an amorphous composite structure, the coating and interface porosity is ≤0.7%, the coating / substrate interface bonding strength is ≥47MPa, the coating surface hardness is ≥420HV1, the sliding friction test wear is ≤1.4 micrograms per square centimeter per hour, and the 50g / L sodium chloride salt spray resistance test corrosion weight loss is ≤0.4 micrograms per square centimeter per hour.

[0117] The stainless steel coating material has an amorphous composite structure and a series of excellent performance parameters, which together constitute the significant advantages of this material in many application fields. The following is a specific analysis of its advantages:

[0118] Low porosity: The porosity of the coating and interface is ≤0.7%, indicating that the coating has high density, effectively preventing the penetration of corrosive media and harmful substances, and improving the corrosion resistance and service life of the coating.

[0119] Strong interface bonding: The coating / substrate interface bonding strength is ≥47MPa, which ensures a strong bond between the coating and the substrate and avoids performance degradation caused by shedding or peeling of the coating during use.

[0120] High hardness: The surface hardness of the coating is ≥420HV1, which is much higher than the hardness of ordinary stainless steel. This makes the coating have excellent scratch and wear resistance and can maintain surface integrity under harsh working conditions.

[0121] Low wear: The wear in the sliding friction test is ≤1.4 micrograms per square centimeter per hour, indicating that the coating wears very little during the friction process, extending the service life of the coating and reducing maintenance costs.

[0122] Salt spray corrosion resistance: 50g / L sodium chloride salt spray test corrosion weight loss ≤ 0.4 micrograms per square centimeter per hour. This excellent salt spray resistance shows that the coating has excellent corrosion resistance in marine environments or other salty environments and can protect the substrate from corrosion.

[0123] The amorphous composite structure combines the high hardness, high strength and excellent corrosion resistance of amorphous materials with the good plasticity and processing properties of crystalline materials, so that the coating material has a certain toughness and plasticity while maintaining high hardness and wear resistance. The amorphous structure also gives the coating material some unique physical and chemical properties, such as lower friction coefficient, higher thermal stability and radiation resistance, which play an important role in specific applications.

[0124] In summary, the prepared stainless steel coating material has an amorphous composite structure and has significant advantages such as low porosity, strong interface bonding, high hardness, low wear, and excellent corrosion resistance. These advantages make the material have broad market prospects and application value in multiple application fields.

[0125] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a wear-resistant stainless steel amorphous composite coating material, It is characterized in that The following steps are involved: An aluminum alloy substrate is used as a substrate, and after surface treatment, a liquid metal atomization method is used to spray on the surface of the substrate to form protrusions, and then the protrusions are hardened to obtain an aluminum alloy substrate to be sprayed; A stainless steel-aluminum alloy composite crystal layer is formed on the surface of the aluminum alloy substrate to be sprayed by a plasma spraying method, and then a stainless steel amorphous layer is prepared on the surface of the stainless steel-aluminum alloy composite crystal layer by a cold spraying method. The stainless steel amorphous layer is then microcrystallized to obtain a wear-resistant stainless steel amorphous composite coating material.

2. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The grade of the aluminum alloy is 2017 or 2024.

3. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The surface treatment is to remove burrs on the surface of the aluminum alloy substrate by a magnetic grinding method, the magnetic abrasive is an iron-based powder with a surface hardness of ≥HB180, the magnetic brush rotates at a speed of 130 to 150 rpm, and the surface roughness of the substrate after grinding is ≤Ra0.04 microns.

4. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The liquid metal atomization method specifically comprises: The same grade of aluminum alloy as the substrate is used as the raw material, argon gas at 560-630°C is used as the power source, the ejection speed is 180-220 m / s, the metal droplets are air-cooled on the surface of the substrate, and finally protrusions are formed on the surface of the substrate with an arrangement density of 3200-3500 per square millimeter.

5. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The hardening treatment of the protrusions comprises: The substrate surface is convexly heated to 530-550°C and then water-cooled.

6. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The method of using a plasma spraying method to spray a stainless steel-aluminum alloy composite crystal layer on the surface of an aluminum alloy substrate to be sprayed comprises: Plasma spraying uses 130-150 micron 2017 or 2024 aluminum alloy powder and 110-130 micron stainless steel powder as raw materials, the mass percentage of aluminum alloy powder and stainless steel powder is (19-25): (75-81), the spraying distance is 32-38 mm, the argon gas flow rate is 47-55 liters per minute, and the thickness of the stainless steel-aluminum alloy composite crystal layer is 110-140 microns.

7. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The method of preparing a stainless steel amorphous layer on the surface of the stainless steel-aluminum alloy composite crystal layer by a cold spraying method comprises: Using the cold spraying method, 25-50 micron stainless steel amorphous powder is used as raw material, and a 110-130 micron thick amorphous layer is sprayed on the surface of the composite crystal layer at 20-28°C. The compressed gas is nitrogen and the speed is 500-700 m / s.

8. The method for preparing the wear-resistant stainless steel amorphous composite coating material according to claim 1, It is characterized in that The microcrystallization treatment of the stainless steel amorphous layer comprises: The coating is crystallized by heat treatment, and is kept at 360-430°C for 45-63 minutes, and then air-cooled.

9. A wear-resistant stainless steel amorphous composite coating material, It is characterized in that The coating is prepared by the method for preparing the wear-resistant stainless steel amorphous composite coating material according to any one of claims 1 to 8.

10. The wear-resistant stainless steel amorphous composite coating material according to claim 9, It is characterized in that The prepared stainless steel coating material has an amorphous composite structure, the coating and interface porosity is ≤0.7%, the coating / substrate interface bonding strength is ≥47MPa, the coating surface hardness is ≥420HV1, the sliding friction test wear is ≤1.4 micrograms per square centimeter per hour, and the 50g / L sodium chloride salt spray test corrosion weight loss is ≤0.4 micrograms per square centimeter per hour.

Citation Information

Cited By

  • Bionic dentate interlaced interlocking structure coating as well as preparation method and application of bionic dentate interlaced interlocking structure coating

    CN120272901A

  • Preparation method of high-strength fitting with high-temperature-resistant coating

    CN120738590A