High-strength corrosion-resistant eccentric reducing pipe and preparation method thereof
Through stamping, nickel plating, boron seepage and modified composite paint spraying technology, the leakage problem of eccentric reducer tubes under stress and corrosion is solved, and its wear resistance and corrosion resistance are improved, which significantly reduces the incidence of accidents.
Patent Information
- Application Number
- CN202411053931.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
AI Technical Summary
Existing eccentric reducer tubes are prone to leakage under stress shock and corrosion, and lack wear resistance and corrosion resistance, resulting in frequent accidents.
The eccentric reducer tube matrix was prepared by stamping method, and after nickel plating and boron dehydration treatment, modified composite paint, including aluminum chromium phosphate and modified nanosilicon dioxide, to form a high-strength, corrosion-resistant surface coating.
It significantly improves the hardness, impact resistance and wear resistance of the eccentric reducer tube, enhances the adhesion and chemical stability of the surface coating, reduces corrosion and wear, and reduces leakage risks.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of eccentric reducers, in particular to a high-strength corrosion-resistant eccentric reducer and a preparation method thereof. Background Art
[0002] An eccentric reducer is a pipe fitting used at the diameter change point of a pipe. Its cross-sectional shape is different from that of a conventional round pipe, and the diameter or wall thickness of the pipe changes on the axis. An eccentric reducer can effectively reduce the flow resistance of the fluid in the pipe, and at the same time can achieve uniform distribution of the flow rate, which is conducive to exhaust or drainage, and is easy to start and maintain. It is commonly used in various heating furnaces, regulating valves, feeders and other equipment, and is an important component second only to elbows. However, due to the influence of the molding process, the eccentric reducer has uneven wall thickness, and after being subjected to long-term stress shock, leakage occurs at welding points or weak parts; in addition, when the fluid flows through the reducer, the fluid flow rate will accelerate. Affected by the fluid properties and fluid flow rate, the eccentric reducer is more susceptible to corrosion, wear, and leakage. Therefore, it is necessary to prepare a more wear-resistant, corrosion-resistant, and high-strength eccentric reducer to reduce the occurrence of accidents. Summary of the invention
[0003] The purpose of the present invention is to provide a high-strength corrosion-resistant eccentric reducer and a preparation method thereof, so as to solve the problems of insufficient wear resistance, insufficient corrosion resistance and insufficient strength of the current eccentric reducer.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0006] Punching out an eccentric reducer matrix from a steel pipe by a punching method, grinding, pickling, washing, and drying the eccentric reducer matrix to obtain a pretreated eccentric reducer;
[0007] The pretreated reducer is placed in an electroplating solution to plate a layer of nickel on its surface, and then buried in a boronizing agent to obtain a boronized eccentric reducer;
[0008] The composite paint is sprayed on the boronized eccentric reducer with a spraying pressure of 0.2-0.3 MPa, a spraying distance of 18-22 cm, a coating thickness of 45-55 μm, and cured at room temperature for 5-7 hours, heated to 180-220°C, cured for 2-4 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0009] As a limitation of the present invention, the specific method for preparing the boronized eccentric reducer is:
[0010] Mix nickel sulfate, nickel chloride, boric acid and deionized water, stir evenly to fully dissolve, and obtain a mixed solution. Mix the mixed solution with sodium dodecyl sulfate in a mass ratio of 1:(0.04-0.06), stir evenly, and obtain an electroplating solution.
[0011] The pre-treated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The current density during electroplating is 1.5-2.5A / dm 2 The electroplating time is 20 to 40 minutes. After the electroplating is completed, the reducer is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0012] Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed and stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and the mixture is kept at 890-910° C. for 3-5 hours to obtain a boronized eccentric reducer.
[0013] As a limitation of the present invention, the preparation method of the composite paint is:
[0014] Phosphoric acid, aluminum hydroxide and deionized water are mixed, reacted at 110-120° C. and 30-50 rpm for 25-35 minutes to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide at a mass ratio of 1:(14-15), reacted at 110-120° C. and 30-50 rpm for 15-25 minutes, and dried after the reaction is completed to obtain aluminum chromium phosphate;
[0015] The coupling agent, ethanol and deionized water are mixed in a mass ratio of 1: (0.4-0.6): 1, and reacted at 28-32°C and 50-70rpm for 40-50min to obtain a coupling agent hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water are evenly mixed, and ultrasonically dispersed for 15-25min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the coupling agent hydrolyzate are mixed in a mass ratio of (4-6): 1, and reacted at 60-70°C and 50-70rpm for 50-70min, and perfluorodecyltrimethoxysilane in an amount of 2.8% to 3.0% by mass of the nano-silicon dioxide dispersion is added, and the reaction is continued for 170-190min to obtain a modified nano-silicon dioxide solution;
[0016] The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine are mixed and stirred evenly to obtain a composite paint.
[0017] As a limitation of the present invention, the mass ratio of the nickel sulfate, nickel chloride, boric acid and deionized water is (23-25):(1-3):(3-4):(68-72).
[0018] As a limitation of the present invention, the mass ratio of boron carbide, potassium fluoroborate, silicon carbide and activated carbon is 1:(4-6):(90-94):(1-3).
[0019] As a limitation of the present invention, the mass ratio of the phosphoric acid, aluminum hydroxide and deionized water is (45-47):(8-10):(17-19).
[0020] As a limitation of the present invention, the mass ratio of the nano-silicon dioxide, glacial acetic acid and deionized water is 1:(4-6):(93-95).
[0021] As a limitation of the present invention, the mass ratio of the modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine is (4-6):(3-5):(48-52):(0.4-0.6).
[0022] The beneficial effects achieved by the present invention are as follows: nickel is a medium-strength reducing agent with a standard potential of -0.25V. The nickel-plated layer is a cathode plating layer for iron, which can effectively protect carbon steel from corrosion. Boriding technology is a surface heat treatment technology. After boriding treatment, the hardness and wear resistance of steel can be significantly improved. However, the FeB generated by direct boriding is brittle, which makes it easy for the boriding layer to peel off from the surface of the workpiece, and has poor thermal shock resistance and high-temperature oxidation resistance. After the surface of steel is nickel-plated and then borided, the phase composition of the boriding layer changes to Ni2B and (Fe, Ni)2B, Fe2B phase and γ-(Fe, Ni) phase. Compared with the FeB generated by direct boriding, the toughness is higher and the impact resistance is better. Moreover, the mutual diffusion process between the boriding layer of steel and the nickel-boriding layer will effectively improve the bonding force between the nickel-boriding layer and the substrate. Aluminum chromium phosphate is a pigment containing chromium ions, which itself has a certain hardness and corrosion resistance. At high temperatures, it can also be transformed into an amorphous substance to block the micropores on the surface and make the coating more dense. After modification, fluorine and silicon are introduced into nano-silicon dioxide, which reduces the surface energy of nano-silicon dioxide particles. Fluorocarbon resin contains a large number of fluorine-carbon bonds, which have excellent chemical stability and extremely low surface energy when combined with modified nano-silicon dioxide, showing good corrosion resistance and weather resistance. DETAILED DESCRIPTION
[0023] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0024] Nano-silica (S817567), perfluorodecyltrimethoxysilane (T820162), and coupling agent (KH-570) were provided by Shanghai McLean, ethylenediamine (10009518) was provided by Sinopharm Group, and silicone defoaming agent (BYK-141) was provided by Shanghai Buding. The steel pipe is made of Q235 steel.
[0025] Steel pipe chemical composition analysis table (wt%)
[0026] element Fe C Mn Si P S content 99.46 0.12 0.15 0.18 0.04 0.05
[0027] Example 1: A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0028] Step 1: Preprocessing
[0029] The eccentric reducer matrix is punched out of the steel pipe by punching and expanding the diameter, and the eccentric reducer matrix is polished. After polishing, the surface is pickled with 23% hydrochloric acid, and then rinsed with deionized water. After rinsing, the temperature is raised to 420°C, kept warm for 30 minutes, and cooled to room temperature to obtain a pretreated eccentric reducer.
[0030] Step 2: Prepare the plating solution
[0031] Nickel sulfate, nickel chloride, boric acid and deionized water are mixed in a mass ratio of 24:2:3.5:70, stirred evenly to fully dissolve, and a mixed solution is obtained. The mixed solution is mixed with sodium dodecyl sulfate in a mass ratio of 1:0.05, stirred evenly, and an electroplating solution is obtained.
[0032] Step 3: Nickel plating
[0033] The pretreated eccentric reducer and pure nickel plate are placed in the electroplating solution, and the pretreated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The electroplating current density is 2A / dm 2 The electroplating time is 30 minutes. After the electroplating is completed, it is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0034] Step 4: Boriding
[0035] Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed in a mass ratio of 1:5:92:2, stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and kept warm at 900°C for 4 hours to obtain a boronized eccentric reducer.
[0036] Step 5: Prepare the composite paint
[0037] Phosphoric acid, aluminum hydroxide and deionized water are mixed in a mass ratio of 46:9:18, reacted at 115° C. and 40 rpm for 30 min to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide in a mass ratio of 1:14.5, reacted at 115° C. and 40 rpm for 20 min, and dried after the reaction is completed to obtain aluminum chromium phosphate;
[0038] KH-570, ethanol and deionized water were mixed in a mass ratio of 1:0.5:1, and reacted at 30°C and 60rpm for 45min to obtain a KH-570 hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water were evenly mixed in a mass ratio of 1:5:94, and ultrasonically dispersed for 20min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the KH-570 hydrolyzate were mixed in a mass ratio of 5:1, and reacted at 65°C and 60rpm for 60min, and perfluorodecyltrimethoxysilane in an amount of 2.8% to 3.0% by mass of the nano-silicon dioxide dispersion was added, and the reaction was continued for 180min to obtain a modified nano-silicon dioxide solution;
[0039] The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine were mixed in a mass ratio of 5:4:50:0.5, stirred evenly, and a composite paint was obtained.
[0040] Step 6: Apply composite paint
[0041] The composite paint was sprayed on the boronized eccentric reducer with a spraying pressure of 0.25 MPa, a spraying distance of 20 cm, a coating thickness of 50 μm, and cured at room temperature for 6 hours, heated to 200°C, cured for 3 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0042] Example 2: A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0043] Step 1: Preprocessing
[0044] The eccentric reducer matrix is punched out of the steel pipe by punching and expanding the diameter, and the eccentric reducer matrix is polished. After polishing, the surface is pickled with 23% hydrochloric acid, and then rinsed with deionized water. After rinsing, the temperature is raised to 420°C, kept warm for 30 minutes, and cooled to room temperature to obtain a pretreated eccentric reducer.
[0045] Step 2: Prepare the plating solution
[0046] Nickel sulfate, nickel chloride, boric acid and deionized water are mixed in a mass ratio of 24:2:3.5:70, stirred evenly to fully dissolve, and a mixed solution is obtained. The mixed solution is mixed with sodium dodecyl sulfate in a mass ratio of 1:0.05, stirred evenly, and an electroplating solution is obtained.
[0047] Step 3: Nickel plating
[0048] The pretreated eccentric reducer and pure nickel plate are placed in the electroplating solution, and the pretreated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The electroplating current density is 2.5A / dm 2 The electroplating time is 30 minutes. After the electroplating is completed, it is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0049] Step 4: Boriding
[0050] Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed in a mass ratio of 1:6:94:3, stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and kept warm at 900° C. for 4 hours to obtain a boronized eccentric reducer.
[0051] Step 5: Prepare the composite paint
[0052] Phosphoric acid, aluminum hydroxide and deionized water are mixed in a mass ratio of 46:9:18, reacted at 115° C. and 40 rpm for 30 min to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide in a mass ratio of 1:14.5, reacted at 115° C. and 40 rpm for 20 min, and dried after the reaction is completed to obtain aluminum chromium phosphate;
[0053] KH-570, ethanol and deionized water were mixed in a mass ratio of 1:0.5:1, and reacted at 30°C and 60rpm for 45min to obtain a KH-570 hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water were evenly mixed in a mass ratio of 1:5:94, and ultrasonically dispersed for 20min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the KH-570 hydrolyzate were mixed in a mass ratio of 5:1, and reacted at 65°C and 60rpm for 60min, and perfluorodecyltrimethoxysilane with a mass fraction of 2.8% to 3.0% of the nano-silicon dioxide dispersion was added, and the reaction was continued for 180min to obtain a modified nano-silicon dioxide solution;
[0054] The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine were mixed in a mass ratio of 6:5:52:0.6, stirred evenly, and a composite paint was obtained.
[0055] Step 6: Apply composite paint
[0056] The composite paint was sprayed on the boronized eccentric reducer with a spraying pressure of 0.25 MPa, a spraying distance of 20 cm, a coating thickness of 50 μm, and cured at room temperature for 6 hours, heated to 200°C, cured for 3 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0057] Example 3: A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0058] Step 1: Preprocessing
[0059] The eccentric reducer matrix is punched out of the steel pipe by punching and expanding the diameter, and the eccentric reducer matrix is polished. After polishing, the surface is pickled with 23% hydrochloric acid, and then rinsed with deionized water. After rinsing, the temperature is raised to 420°C, kept warm for 30 minutes, and cooled to room temperature to obtain a pretreated eccentric reducer.
[0060] Step 2: Prepare the plating solution
[0061] Nickel sulfate, nickel chloride, boric acid and deionized water are mixed in a mass ratio of 24:2:3.5:70, stirred evenly to fully dissolve, and a mixed solution is obtained. The mixed solution is mixed with sodium dodecyl sulfate in a mass ratio of 1:0.05, stirred evenly, and an electroplating solution is obtained.
[0062] Step 3: Nickel plating
[0063] The pretreated eccentric reducer and pure nickel plate are placed in the electroplating solution, and the pretreated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The electroplating current density is 1.5A / dm 2 The electroplating time is 30 minutes. After the electroplating is completed, it is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0064] Step 4: Boriding
[0065] Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed in a mass ratio of 1:4:90:1, stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and kept warm at 900° C. for 4 hours to obtain a boronized eccentric reducer.
[0066] Step 5: Prepare the composite paint
[0067] Phosphoric acid, aluminum hydroxide and deionized water are mixed in a mass ratio of 46:9:18, reacted at 115° C. and 40 rpm for 30 min to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide in a mass ratio of 1:14.5, reacted at 115° C. and 40 rpm for 20 min, and dried after the reaction is completed to obtain aluminum chromium phosphate;
[0068] KH-570, ethanol and deionized water were mixed in a mass ratio of 1:0.5:1, and reacted at 30°C and 60rpm for 45min to obtain a KH-570 hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water were evenly mixed in a mass ratio of 1:5:94, and ultrasonically dispersed for 20min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the KH-570 hydrolyzate were mixed in a mass ratio of 5:1, and reacted at 65°C and 60rpm for 60min, and perfluorodecyltrimethoxysilane with a mass fraction of 2.8% to 3.0% of the nano-silicon dioxide dispersion was added, and the reaction was continued for 180min to obtain a modified nano-silicon dioxide solution;
[0069] The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine were mixed in a mass ratio of 4:3:48:0.4, stirred evenly, and a composite paint was obtained.
[0070] Step 6: Apply composite paint
[0071] The composite paint was sprayed on the boronized eccentric reducer with a spraying pressure of 0.25 MPa, a spraying distance of 20 cm, a coating thickness of 50 μm, and cured at room temperature for 6 hours, heated to 200°C, cured for 3 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0072] Based on Example 1, a control experiment was carried out, specifically Comparative Example 1 and Comparative Example 2, as described below:
[0073] Comparative Example 1: No boronizing treatment was performed, and other conditions were the same as those in Example 1.
[0074] A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0075] Step 1: Preprocessing
[0076] The eccentric reducer matrix is punched out of the steel pipe by punching and expanding the diameter, and the eccentric reducer matrix is polished. After polishing, the surface is pickled with 23% hydrochloric acid, and then rinsed with deionized water. After rinsing, the temperature is raised to 420°C, kept warm for 30 minutes, and cooled to room temperature to obtain a pretreated eccentric reducer.
[0077] Step 2: Prepare the plating solution
[0078] Nickel sulfate, nickel chloride, boric acid and deionized water are mixed in a mass ratio of 24:2:3.5:70, stirred evenly to fully dissolve, and a mixed solution is obtained. The mixed solution is mixed with sodium dodecyl sulfate in a mass ratio of 1:0.05, stirred evenly, and an electroplating solution is obtained.
[0079] Step 3: Nickel plating
[0080] The pretreated eccentric reducer and pure nickel plate are placed in the electroplating solution, and the pretreated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The electroplating current density is 2A / dm 2 The electroplating time is 30 minutes. After the electroplating is completed, it is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0081] Step 4: Prepare the composite paint
[0082] Phosphoric acid, aluminum hydroxide and deionized water are mixed in a mass ratio of 46:9:18, reacted at 115° C. and 40 rpm for 30 min to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide in a mass ratio of 1:14.5, reacted at 115° C. and 40 rpm for 20 min, and dried after the reaction is completed to obtain aluminum chromium phosphate;
[0083] KH-570, ethanol and deionized water were mixed in a mass ratio of 1:0.5:1, and reacted at 30°C and 60rpm for 45min to obtain a KH-570 hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water were evenly mixed in a mass ratio of 1:5:94, and ultrasonically dispersed for 20min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the KH-570 hydrolyzate were mixed in a mass ratio of 5:1, and reacted at 65°C and 60rpm for 60min, and perfluorodecyltrimethoxysilane in an amount of 2.8% to 3.0% by mass of the nano-silicon dioxide dispersion was added, and the reaction was continued for 180min to obtain a modified nano-silicon dioxide solution;
[0084] The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine were mixed in a mass ratio of 5:4:50:0.5, stirred evenly, and a composite paint was obtained.
[0085] Step 5: Apply composite paint
[0086] The composite paint was sprayed on the nickel-plated eccentric reducer with a spraying pressure of 0.25 MPa, a spraying distance of 20 cm, a coating thickness of 50 μm, and cured at room temperature for 6 hours, heated to 200°C, cured for 3 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0087] Comparative Example 2: No aluminum chromium phosphate and modified silica were added to the composite paint, and the remaining conditions were the same as in Example 1.
[0088] A method for preparing a high-strength, corrosion-resistant eccentric reducer, the preparation method comprising:
[0089] Step 1: Preprocessing
[0090] The eccentric reducer matrix is punched out of the steel pipe by punching and expanding the diameter, and the eccentric reducer matrix is polished. After polishing, the surface is pickled with 23% hydrochloric acid, and then rinsed with deionized water. After rinsing, the temperature is raised to 420°C, kept warm for 30 minutes, and cooled to room temperature to obtain a pretreated eccentric reducer.
[0091] Step 2: Prepare the plating solution
[0092] Nickel sulfate, nickel chloride, boric acid and deionized water are mixed in a mass ratio of 24:2:3.5:70, stirred evenly to fully dissolve to obtain a mixed solution, 0.05 times the mass of the mixed solution of sodium dodecyl sulfate is added to the mixed solution, stirred evenly to obtain an electroplating solution.
[0093] Step 3: Nickel plating
[0094] The pretreated eccentric reducer and pure nickel plate are placed in the electroplating solution, and the pretreated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The electroplating current density is 2A / dm 2 The electroplating time is 30 minutes. After the electroplating is completed, it is taken out and dried naturally to obtain a nickel-plated eccentric reducer.
[0095] Step 4: Boriding
[0096] Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed in a mass ratio of 1:5:92:2, stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and kept warm at 900°C for 4 hours to obtain a boronized eccentric reducer.
[0097] Step 5: Prepare the composite paint
[0098] The self-crosslinking water-based fluorocarbon resin and ethylenediamine were mixed in a mass ratio of 50:0.5, and stirred evenly to obtain a composite paint.
[0099] Step 6: Apply composite paint
[0100] The composite paint was sprayed on the boronized eccentric reducer with a spraying pressure of 0.25 MPa, a spraying distance of 20 cm, a coating thickness of 50 μm, and cured at room temperature for 6 hours, heated to 200°C, cured for 3 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
[0101] Detection experiment:
[0102] Adhesion test
[0103] The steel pipes were processed according to the preparation methods of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively, to obtain 5 different high-strength corrosion-resistant steel pipes required for the test.
[0104] According to the "Scratch Test for Paint and Varnish Films" (GB / T 9286-1998), the coating adhesion is tested by grid division. Grid division is performed on the prepared coating, and then tape is adhered to the grid division and the tape is pulled up evenly. The damage of the grid is observed with a magnifying glass, and the adhesion of the coating is judged by comparing with the standard.
[0105] Corrosion resistance test
[0106] The steel pipes were processed according to the preparation methods of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively, to obtain 5 different high-strength corrosion-resistant steel pipes required for the test.
[0107] According to the "Determination of Neutral Salt Spray Resistance of Paints and Varnishes" (GB / T 1771-2007), the coating is subjected to a neutral salt spray test using 5% NaCl. The prepared samples are placed in a salt spray chamber, and the samples are observed at regular intervals to analyze their corrosion resistance.
[0108] Impact resistance test
[0109] The steel pipes were processed according to the preparation methods of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively, to obtain 5 different high-strength corrosion-resistant steel pipes required for the test.
[0110] According to the "Determination of Impact Resistance of Paint Film" (GB / T 1732-1993), fix the sample on the workbench of the impact tester, hit the sample with a heavy hammer, and observe the surface condition of the sample.
[0111] Wear resistance test
[0112] The steel pipes were processed according to the preparation methods of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively, to obtain 5 different high-strength corrosion-resistant steel pipes required for the test.
[0113] According to the "Determination of Abrasion Resistance of Paint Film" (GB 1768-79), the prepared sample is fixed on the working turntable of the abrasion tester, and a load of 2000N is applied to the sample. After reaching the specified number of wear-resistant revolutions, the wear of the sample surface coating is observed and the weight loss of the sample is measured.
[0114] High strength corrosion resistant steel pipe test results table
[0115] Adhesion Corrosion resistance Abrasion weight loss (mg) Impact strength (kg cm) Experimental Example 1 Level 0 90d No abnormality 4.2 ≥50 Experimental Example 2 Level 0 90d No abnormality 4.2 ≥50 Experimental Example 3 Level 0 90d slight bubbling 4.4 ≥45 Comparative Example 1 Level 1 90d: blistering, no shedding 6.3 ≥40 Comparative Example 2 Level 1 90d has bubbles and falls off 4.5 ≥45
[0116] Conclusion: It can be seen from the experiment that the sample prepared by the preparation method of Example 1 performs better than the samples prepared by the preparation methods of Comparative Examples 1 and 2 in the adhesion, impact resistance and wear resistance tests. Compared with Example 1, Comparative Example 1 is not subjected to boronization treatment, and the increase in wear loss and the significant decrease in impact strength are shown in the experiment. The composite paint used in Comparative Example 2 does not add aluminum chromium phosphate and modified nano-silicon dioxide, and the water resistance and corrosion resistance are significantly reduced in the experiment. Therefore, the high-strength corrosion-resistant eccentric reducer of the present invention does have the characteristics of high strength, wear resistance and corrosion resistance.
[0117] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength, corrosion-resistant eccentric reducer, characterized in that: The preparation method is: Punching out an eccentric reducer matrix from a steel pipe by a punching method, grinding, pickling, washing, and drying the eccentric reducer matrix to obtain a pretreated eccentric reducer; The pretreated eccentric reducer is placed in an electroplating solution to plate a layer of nickel on its surface, and then buried in a boronizing agent for boronizing treatment to obtain a boronized eccentric reducer; The composite paint is sprayed on the boronized eccentric reducer with a spraying pressure of 0.2-0.3 MPa, a spraying distance of 18-22 cm, a coating thickness of 10-20 μm, and cured at room temperature for 5-7 hours, heated to 180-220°C, cured for 2-4 hours, and naturally cooled to obtain a high-strength, corrosion-resistant eccentric reducer.
2. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 1, characterized in that: The specific method for preparing the boronized eccentric reducer is: Mix nickel sulfate, nickel chloride, boric acid and deionized water, stir evenly to fully dissolve, and obtain a mixed solution. Mix the mixed solution with sodium dodecyl sulfate in a mass ratio of 1:(0.04-0.06), stir evenly, and obtain an electroplating solution. The pre-treated eccentric reducer is used as the cathode and the pure nickel plate is used as the anode for electroplating. The current density during electroplating is 1.5-2.5A / dm 2 The electroplating time is 20 to 40 minutes. After the electroplating is completed, the reducer is taken out and dried naturally to obtain a nickel-plated eccentric reducer. Boron carbide, potassium fluoroborate, silicon carbide and activated carbon are mixed and stirred evenly to obtain a boronizing agent, a nickel-plated eccentric reducer is buried in the boronizing agent, and the mixture is kept at 890-910° C. for 3-5 hours to obtain a boronized eccentric reducer.
3. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 1, characterized in that: The preparation method of the composite paint is: Phosphoric acid, aluminum hydroxide and deionized water are mixed, reacted at 110-120° C. and 30-50 rpm for 25-35 minutes to obtain an aluminum phosphate solution, the aluminum phosphate solution is mixed with chromium trioxide at a mass ratio of 1:(14-15), reacted at 110-120° C. and 30-50 rpm for 15-25 minutes, and dried after the reaction is completed to obtain aluminum chromium phosphate; The coupling agent, ethanol and deionized water are mixed in a mass ratio of 1: (0.4-0.6): 1, and reacted at 28-32°C and 50-70rpm for 40-50min to obtain a coupling agent hydrolyzate; nano-silicon dioxide, glacial acetic acid and deionized water are evenly mixed, and ultrasonically dispersed for 15-25min to obtain a nano-silicon dioxide dispersion; the nano-silicon dioxide dispersion and the coupling agent hydrolyzate are mixed in a mass ratio of (4-6): 1, and reacted at 60-70°C and 50-70rpm for 50-70min, and perfluorodecyltrimethoxysilane in an amount of 2.8% to 3.0% by mass of the nano-silicon dioxide dispersion is added, and the reaction is continued for 170-190min to obtain a modified nano-silicon dioxide solution; The modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine are mixed and stirred evenly to obtain a composite paint.
4. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 2, characterized in that: The mass ratio of nickel sulfate, nickel chloride, boric acid and deionized water is (23-25):(1-3):(3-4):(68-72).
5. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 2, characterized in that: The mass ratio of boron carbide, potassium fluoroborate, silicon carbide and activated carbon is 1:(4-6):(90-94):(1-3).
6. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 3, characterized in that: The mass ratio of phosphoric acid, aluminum hydroxide and deionized water is (45-47):(8-10):(17-19).
7. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 3, characterized in that: The mass ratio of nano-silicon dioxide, glacial acetic acid and deionized water is 1:(4-6):(93-95).
8. The method for preparing a high-strength, corrosion-resistant eccentric reducer according to claim 3, characterized in that: The mass ratio of modified nano-silica solution, aluminum chromium phosphate, self-crosslinking water-based fluorocarbon resin and ethylenediamine is (4-6):(3-5):(48-52):(0.4-0.6).