Curable resin composition for sealing material for film liquid crystal panel, and film liquid crystal panel having end sealing by using same
The curable resin composition formed by a specific combination of multifunctional compounds is solved by solving the problem of liquid crystal contamination in the useability and humid and hot environment of the film liquid crystal panel sealing material in an uncured state, and high adhesion and impact resistance are achieved.
Patent Information
- Application Number
- CN202380037542.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-27
- Filing Date
- 2023-09-20
- Publication Date
- 2024-11-26
AI Technical Summary
The existing film liquid crystal panel sealing materials are poorly used in an uncured state, are prone to liquid crystal contamination, and lead to liquid crystal orientation disorder in harsh and humid environments, and lack adhesion and impact resistance to the curved film substrate.
Combining polyfunctional mercaptan compounds with specific polyfunctional urethane (meth)acrylate compounds, polyfunctional (methyl)allyl compounds and monofunctional (methyl)allyl compounds , a curable resin composition with high flexibility and high water resistance is formed through thiol-ene reaction, which is used for sealing materials to ensure that the liquid crystal does not contaminate in the uncured state and maintain the liquid crystal orientation stable under a humid and heat environment.
It achieves high useability and non-liquid crystal contamination in the uncured state, ensuring that the sealing material does not cause liquid crystal orientation disorder in harsh humid and heat environments, and has high adhesion and impact resistance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin composition for a sealing material for a film liquid crystal panel. In detail, it relates to a curable resin composition for forming a sealing material for a film liquid crystal, which has excellent usability in an uncured state, and does not contaminate the liquid crystal even if it comes into contact with the liquid crystal, and its cured product does not cause the orientation disorder of the liquid crystal even in a harsh hot and humid environment. It has excellent adhesion to a curved film substrate and further has high impact resistance that does not peel off from the film substrate even if an impact is applied. In addition, it also relates to a film liquid crystal panel using a sealing material composed of the curable resin composition. Background Art
[0002] Liquid crystal panels are widely used in image display of various electronic devices such as mobile phones and personal computers. Liquid crystal panels generally have: a pair of glass substrates with electrodes provided on the surface, a frame-shaped sealing material sandwiched between the glass substrates, and a liquid crystal layer surrounded by the sealing material.
[0003] In the past, a photocurable acrylic resin composition was used in the sealing material. However, although the conventional acrylic resin composition has excellent operability and productivity, a large amount of outgassing (out gas) will be generated during the manufacturing process, resulting in a problem of decreased adhesion between the sealing material and the substrate. In addition, the sealing material is also required to protect the liquid crystal under a harsh hot and humid environment, but the conventional sealing material composed of the acrylic resin composition has low water barrier or the sealing material is easy to decompose, and there is a problem of liquid crystal contamination caused by moisture or sealing material decomposition products under hot and humid environments, resulting in a problem of disordered orientation of the liquid crystal.
[0004] In view of the above problems, it is known that by using a resin composition containing a thiol monomer having a thiol group and an olefin monomer having a carbon-carbon double bond, the occurrence of degassing can be suppressed and the adhesion of the sealing material can be improved (Patent Documents 1 and 2). In addition, Patent Documents 1 and 2 also confirm that by improving the water resistance and durability of the sealing material, even in a harsh hot and humid environment, the orientation disorder of the liquid crystal will not occur when the sealing material is in contact with the liquid crystal.
[0005] However, in the manufacture of liquid crystal panels, there is a process in which the resin composition used as a sealing material comes into contact with liquid crystal in an uncured state. However, in this process, the sealing materials of Patent Documents 1 and 2 have a problem in which the resin components dissolve into the liquid crystal and cause liquid crystal contamination, resulting in display failure.
[0006] In addition, in recent years, film liquid crystal panels using flexible film materials as substrates have attracted attention and have been developed. The sealing material used for the film liquid crystal panel is different from the sealing material used for the rigid glass substrate, and is required to have rich softness and toughness, and have high adhesion to the curved film substrate. However, the sealing materials of Patent Documents 1 and 2 cannot take into account both softness and toughness, and the adhesion to the curved film substrate is not sufficient.
[0007] In view of the above problems, it is known that by using a resin composition containing a multifunctional thiol compound, a multifunctional urethane (meth) acrylate compound and a multifunctional (meth) allyl compound, even when the curable resin composition is in contact with the liquid crystal in an uncured state, the pollution of the liquid crystal can be suppressed, and the orientation disorder of the liquid crystal will not occur (patent document 3). In addition, the curable resin composition of patent document 3 can be made into a sealing material with high softness and toughness after curing, and excellent compliance to the film substrate.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2016-169298
[0011] Patent Document 2: Japanese Patent Application Publication No. 2017-54084
[0012] Patent Document 3: Japanese Patent Application Publication No. 2021-162680 Summary of the invention
[0013] 1. Technical issues to be resolved
[0014] Electronic devices using film liquid crystal panels are sometimes used in a manner of being carried and transported by users, so the sealing material of the film liquid crystal panel is required to have an impact resistance that will not be peeled off from the film substrate even when subjected to a strong impact. In addition, from the perspective of operability and productivity, it is also required that the resin composition used for the sealing material is stable and has high usability in an uncured state and will not gel over a long period of time. However, the usability of the curable resin composition of the above-mentioned patent document 3 in an uncured state is not sufficient, and there is still room for improvement in impact resistance.
[0015] In view of the above-mentioned actual situation, the present invention is implemented, and its purpose is to provide a curable resin composition for use as a sealing material for a film liquid crystal panel and a film liquid crystal panel using the curable resin composition as a sealing material. The curable resin composition has excellent usability in an uncured state and will not contaminate the liquid crystal even if it comes into contact with the liquid crystal. In addition, its cured product will not cause orientation disorder of the liquid crystal even when it comes into contact with the liquid crystal in a harsh hot and humid environment, and has excellent adhesion to a curved film substrate, and further has high impact resistance that will not peel off from the film substrate even if an impact is applied.
[0016] (II) Technical solution
[0017] The inventors of the present application have repeatedly conducted in-depth research to solve the above-mentioned technical problems, and found that by using a curable resin composition that combines a specific multifunctional urethane (meth) acrylate compound with a specific multifunctional (meth) allyl compound and a specific monofunctional (meth) allyl compound, and further contains a multifunctional thiol compound, it is possible to obtain a film liquid crystal panel sealing material that has excellent usability in an uncured state, and will not contaminate the liquid crystal even if it comes into contact with the liquid crystal, and the cured product will not cause the orientation disorder of the liquid crystal even in a harsh humid and hot environment. In addition, the sealing material has both softness and toughness, excellent adhesion to a curved film substrate, and further has high impact resistance that will not peel off from the film substrate even if an impact is applied, thereby completing the present invention.
[0018] That is, the present invention is the following (1) to (2).
[0019] (1) A curable resin composition for a film liquid crystal panel sealing material, comprising the following components (A) to (D):
[0020] (A) a multifunctional thiol compound having 2 to 6 thiol groups,
[0021] (B) a polyfunctional urethane (meth)acrylate compound having 2 to 3 (meth)acryloyl groups,
[0022] (C) a polyfunctional (meth)allyl compound having 2 to 4 (meth)allyl groups,
[0023] (D) a monofunctional (meth)allyl compound having one (meth)allyl group, and
[0024] (E) a photopolymerization initiator,
[0025] The blending mass ratio of (B) to (C) and (D) is (B) / [(C)+(D)] 0.1~1.0,
[0026] The blending mass ratio of (C) to (D) is (C) / (D) in the range of 0.3 to 3.0.
[0027] The ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bond of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is 0.4 to 3.0.
[0028] (2) A film liquid crystal panel having its edges sealed with the curable resin composition described in (1) above.
[0029] In the present invention, "(meth)allyl compound" refers to a general term for compounds having allyl groups and compounds having methallyl groups, and the same applies to "(meth)acryloyl" and the like. Unless otherwise specified, "○○~××" in the present invention indicating a numerical range is a concept including a lower limit ("○○") and an upper limit ("××"). That is, to be precise, it means "above ○○ and below ××". .
[0030] (III) Beneficial effects
[0031] The present invention can provide a curable resin composition for a sealing material for a film liquid crystal panel, the curable resin composition has excellent usability in an uncured state, and will not contaminate the liquid crystal even if it comes into contact with the liquid crystal, and its cured product will not cause the orientation disorder of the liquid crystal even in a harsh hot and humid environment, and has excellent adhesion to a curved film substrate, and further has high impact resistance that will not peel off from the film substrate even if an impact is applied. In addition, a film liquid crystal panel using the above-mentioned curable resin composition as a sealing material is also provided. DETAILED DESCRIPTION
[0032] The present invention will be described in detail below. The curable resin composition of the present invention is used for a film liquid crystal panel sealing material, and contains the following (A), (B), (C), (D), and (E) as essential components.
[0033] <Multifunctional thiol compound (A)>
[0034] The multifunctional thiol compound (A) is a compound having 2 to 6 thiol groups. The multifunctional thiol compound (A) can be used alone or in combination of two or more. By containing the compound, the thiol-ene reaction with other components can be promoted to improve curability. Compared with the bonds of atoms such as C, O, and N, the bond angle of the formed thioether bond can be flexibly changed, so the softness of the cured product is high, and the adhesion and impact resistance of the sealing material to the curved film substrate can be improved. In addition, the cured product composed of the thioether bond has a high softness of the bond angle, and can be cured at a high density in a manner that atoms are buried in the gaps between the bonds, so the water barrier is high, and it will not be affected by moisture even after the wet heat test, and the orientation disorder of the liquid crystal can be prevented.
[0035] The polyfunctional thiol compound (A) is preferably a compound represented by the following formula 1.
[0036] [Chemical formula 1]
[0037]
[0038] Where a is an integer from 2 to 6, R 1 It is a 2- to 6-valent organic group having 10 to 60 carbon atoms.
[0039] From the perspective of improving the water barrier property of the film liquid crystal panel sealing material and suppressing the orientation disorder even when exposed to a harsh wet heat test, a in the formula is preferably an integer of 3 to 6. If a in the formula is within this range, the curing shrinkage will not increase and the adhesion to the film substrate after curing will not decrease, and a good cured product can be obtained. In addition, from the same perspective, R 1 Preferably, the valence is 3 to 6. 1 The number of carbon atoms is 10 to 60, preferably 10 to 45, and more preferably 12 to 30. 1 When the number of carbon atoms is within this range, the crosslinking density of the cured product of the curable resin composition is sufficient, the sealing material has excellent water barrier properties, and even when exposed to a severe wet heat test, the alignment disorder of the liquid crystal can be suppressed.
[0040] The organic group is a group containing C and may further contain at least one element selected from the group consisting of Si, N, P, O and S. The organic group may also be a polymer having a repeating unit. In addition, in its structure, groups such as ketone groups, ester groups, ether groups, hydroxyl groups, amide groups, thioether groups, isocyanurate groups, and glycoluril groups may also be contained.
[0041] Specific examples of the polyfunctional thiol compound (A) include dipentaerythritol hexa(3-mercaptopropionate), trimethylolpropane tri(2-mercaptoacetate), trimethylolpropane tri(3-mercaptopropionate), trimethylolethane tri(2-mercaptoacetate), trimethylolethane tri(3-mercaptopropionate), pentaerythritol tetra(2-mercaptoacetate), pentaerythritol tetra(3-mercaptopropionate), 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris(3-mercaptopropylthio)propane, 4-mercaptomethyl-1,8 -dimercapto-3,6-dithia-octane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithia-undecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithia-undecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithia-undecane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, 1,3,5-tris(mercaptoethyleneoxy)benzene, tris-[(3-mercaptopropyleneoxy)-ethyl]-isocyanurate, and the like.
[0042] Among the compounds represented by the above formula 1, polyfunctional thiol having a pentaerythritol skeleton, polyfunctional thiol having a dipentaerythritol skeleton, and polyfunctional thiol having an isocyanurate skeleton are preferred.
[0043] Among them, dipentaerythritol hexa(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), and tris-[(3-mercaptopropyleneoxy)-ethyl]-isocyanurate are preferred because they can improve the water barrier properties of the sealing material, suppress the orientation disorder of the liquid crystal even when exposed to harsh heat and humidity tests, and improve the flexibility of the cured product of the curable resin composition, thereby improving the adhesion and impact resistance of the sealing material to the substrate.
[0044] As the polyfunctional thiol compound (A), a commercially available product or a synthesized product may be used. As a synthesis method, it can be obtained by esterification reaction of a polyol such as pentaerythritol with a mercapto group-containing carboxylic acid such as 3-mercaptopropionic acid by a known method.
[0045] <Multifunctional urethane (meth)acrylate compound (B)>
[0046] The multifunctional carbamate (meth) acrylate compound (B) can be obtained by reacting a diisocyanate compound with a polyol compound and a (meth) acrylate compound having a hydroxyl group by a known method. The multifunctional carbamate (meth) acrylate compound (B) can be used alone or in combination of two or more. Due to its high lyophobicity with liquid crystals, the compound can reduce the solubility of the uncured curable resin composition in liquid crystals by containing the compound, and can prevent the contamination of liquid crystals even when in contact with liquid crystals for a long time. In addition, the strong interaction of the hydrogen bonds between the contained carbamate groups and other polar groups can show the toughness of the cured product of the curable resin composition and the adhesion to the substrate, and can improve the adhesion and impact resistance of the sealing material to the curved film substrate. The multifunctional urethane (meth)acrylate compound (B) is a compound having 2 to 3 (meth)acryloyl groups. By setting the number of (meth)acryloyl groups within this range, the cured product of the curable resin composition will not become rigid, and the adhesion and impact resistance of the sealing material to a curved film substrate can be improved.
[0047] The diisocyanate compound can use a known compound. For example, aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates can be listed. Specifically, aliphatic diisocyanates such as pentamethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, hydrogenated diphenyl diisocyanate, and norbornene diisocyanate; aromatic diisocyanates such as xylene diisocyanate, toluene diisocyanate, and diphenylmethane diisocyanate can be listed. Among them, from the perspective of preventing the obtained sealing material from being colored over time, aliphatic diisocyanates and alicyclic diisocyanates are preferred.
[0048] The polyol compound may be a known compound. For example, polyester polyols, polyether polyols, polycarbonate polyols, and polyols composed of hydrocarbons may be cited. From the perspective that the polarity of the multifunctional urethane acrylate compound obtained after the reaction is not too high and that the adhesion and impact resistance of the sealing material to the curved film substrate can be improved, the polyol compound is preferably a divalent diol compound or a trivalent triol compound.
[0049] As the polyester polyol, a compound obtained by condensing a dicarboxylic acid compound with a polyol compound can be used. As the dicarboxylic acid compound, specifically succinic acid, adipic acid, pimelic acid, sebacic acid, etc. can be listed. Among them, adipic acid and pimelic acid are preferred. In addition, as the polyol compound, for example, a diol compound and a triol compound can be listed. As the diol compound, specifically ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, diethylene glycol, dipropylene glycol, etc. can be listed. As the triol compound, specifically glycerol, 1,2,4-butanetriol, trihydroxypropane, etc. can be listed. Among them, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, glycerol are preferred.
[0050] The polyether polyol may be a known compound. Specifically, diol compounds such as polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol; and triol compounds such as polyoxypropylene triol (polyoxypropylentriol) and polyoxyethylene polyoxypropylene triol are listed. Among them, polyethylene glycol, polypropylene glycol, and polyoxypropylene triol are preferred.
[0051] As the polycarbonate polyol, a compound obtained by transesterification of a carbonate diester with a polyol compound can be used. As a carbonate diester, specifically diphenyl carbonate, dimethyl carbonate, diethylene carbonate (diethylene carbonate), etc. can be listed. Among them, diphenyl carbonate is preferred. As a polyol compound, for example, a diol compound and a triol compound can be listed. As a diol compound, specifically ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, diethylene glycol, dipropylene glycol, etc. can be listed. As a triol compound, specifically glycerol, 1,2,4-butanetriol, trihydroxypropane, etc. can be listed. Among them, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, glycerol are preferred.
[0052] The polyol composed of hydrocarbons may be a known compound. Specifically, diol compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, and 1,8-octanediol, and triol compounds such as glycerol, 1,2,4-butanetriol, and trihydroxypropane may be mentioned. Among them, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, and glycerol are preferred.
[0053] The (meth) acrylate compound with hydroxyl group can use known compounds. Specifically, 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, 4-hydroxycyclohexyl (meth) acrylate, 5-hydroxycyclooctyl (meth) acrylate, 2-hydroxy-3-phenyloxypropyl (meth) acrylate, propylene glycol monoacrylate, polyethylene glycol mono(meth) acrylate, polypropylene glycol mono(meth) acrylate, etc. can be used. Among them, from the perspective of preventing the sealing material from being colored over time, and improving the flexibility of the cured product of the curable resin composition, improving the adhesion of the sealing material to the curved film substrate and the impact resistance, 2-hydroxyethyl acrylate and propylene glycol monoacrylate are preferred.
[0054] The weight average molecular weight of the polyfunctional urethane (meth) acrylate compound (B) is preferably 1,000 to 15,000, more preferably 3,000 to 10,000, from the viewpoint of being able to simultaneously achieve that the curable resin composition does not contaminate the liquid crystal even when it comes into contact with the liquid crystal in an uncured state, that the sealing material can suppress the orientation disorder of the liquid crystal even when exposed to a harsh damp heat test, that it has excellent adhesion to a curved film substrate, that it has various properties of impact resistance, and that it is easy to handle. The weight average molecular weight of the urethane (meth) acrylate can be determined by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene.
[0055] <Polyfunctional (meth)allyl compound (C)>
[0056] The multifunctional (meth)allyl compound (C) is a compound having 2 to 4 (meth)allyl groups. The multifunctional (meth)allyl compound (C) can be used alone or in combination of two or more. Since the (meth)allyl compound does not undergo polymerization reaction between the (meth)allyl compounds, it can efficiently form a thioether bond with the thiol compound. Thus, by containing (C), the crosslinking density increases, the toughness of the cured product of the curable resin composition increases, and the adhesion of the sealing material to the curved film substrate can be improved. In addition, the sealing material has excellent water resistance, and since it is not easy to hydrolyze in the humidity test compared with the (meth)acrylic compound, the high water resistance of the sealing material can be maintained in the humidity test, and the orientation disorder of the liquid crystal can be suppressed even when exposed to harsh heat and humidity tests.
[0057] The polyfunctional (meth)allyl compound (C) is preferably a compound represented by the following formula 2.
[0058] [Chemical formula 2]
[0059]
[0060] In the formula, b is an integer of 2 to 4. 2 is a hydrogen atom or a methyl group. 3 It is a di- to tetravalent organic group having 2 to 40 carbon atoms.
[0061] R in the formula 2 R is a hydrogen atom or a methyl group. From the perspective of increasing the flexibility of the cured product of the curable resin composition and improving the adhesion of the sealing material to the substrate, 2 Preferably, a hydrogen atom is used. b is an integer of 2 to 4. By making b within this range, the water barrier property of the sealing material can be improved, and even when exposed to a harsh wet heat test, the orientation disorder can be suppressed, and the toughness of the cured product of the curable resin composition can be improved, and the adhesion of the sealing material to the curved film substrate can be improved. In addition, from the perspective of maintaining the high water barrier property of the cured product of the curable resin composition and the adhesion of the sealing material to the film substrate, while also improving the flexibility and improving the impact resistance of the sealing material, b is preferably 2 to 3, and b is more preferably 2. From the same perspective, R 3 It is 2-4 valent, preferably 2-3 valent, and more preferably 2 valent. 3 The number of carbon atoms is 2 to 40, preferably 2 to 30, and more preferably 2 to 25. 23 When the number of carbon atoms is within this range, the crosslinking density of the cured product of the curable resin composition is sufficient, and the sealing material can obtain good water barrier properties, so that even when exposed to a severe wet heat test, the orientation disorder can be suppressed.
[0062] The organic group refers to a group containing C and further containing at least one element selected from the group consisting of Si, N, P, O and S. The organic group may also be a polymer having a repeating unit. In addition, in its structure, it may also contain groups such as a ketone group, an ester group, an ether group, a hydroxyl group, an amide group, a thioether group, and an isocyanurate group.
[0063] For example, as the compound in which b in the formula is 2, specific examples include di(methyl)allyl 1,4-cyclohexanedicarboxylate, di(methyl)allyl isophthalate, di(methyl)allyl phthalate, di(methyl)allyl hexahydrophthalate, di(methyl)allyl methyl glycidyl isocyanurate, magnolol, di(methyl)allyl diphenylsilane, trihydroxypropane di(methyl)allyl ether, 2,2'-bis(3-(methyl)allyl-4-hydroxyphenyl)propane, 2,2-bis(3-(methyl)allyl-4-allyloxyphenyl)propane, 2,2-bis(3-(methyl)allyl-4-glycidyl ether phenyl)propane, 1,3-di(methyl)allyl-5-glycidyl isocyanurate, and 1,3-di(methyl)allyl isocyanurate.
[0064] Specific examples of the compound wherein b is 3 include triallyl isocyanurate, pentaerythritol tri(meth)allyl ether, glycerol tri(meth)allyl ether, and trihydroxypropane triallyl ether.
[0065] Specific examples of the compound wherein b is 4 include 1,3,4,6-tetra(methyl)allyl glycoluril, 1,3,4,6-tetra(methyl)allyl-3a-methyl glycoluril, pentaerythritol tetra(methyl)allyl ether, and tetra(methyl)allyl ethane oxide.
[0066] Among the above-mentioned (meth)allyl compounds, (meth)allyl compounds having an isocyanurate skeleton and (meth)allyl compounds having a pentaerythritol skeleton are preferred from the viewpoints of preventing the sealing material from being discolored over time, improving the water barrier property of the sealing material, suppressing the orientation disorder even when exposed to a severe heat and humidity test, improving the toughness of the cured product of the curable resin composition, and improving the adhesion to a curved film substrate. Among them, 1,3-diallyl-5-glycidyl isocyanurate, triallyl isocyanurate, pentaerythritol triallyl ether, and pentaerythritol tetraallyl ether are specifically preferred.
[0067] <Monofunctional (meth)allyl compound (D)>
[0068] The monofunctional (meth)allyl compound (D) is a compound having one (meth)allyl group. The monofunctional (meth)allyl compound (D) can be used alone or in combination of two or more. By containing (D), the toughness and high water resistance of the cured product of the curable resin composition can be maintained while the flexibility is greatly improved, and the impact resistance of the sealing material is improved. In addition, the degree of crosslinking in the curing reaction of the curable resin composition can be adjusted to suppress the degree of increase in the viscosity of the uncured product of the curable resin composition, thereby improving the usability of the curable resin composition.
[0069] The monofunctional (meth)allyl compound (D) is preferably a compound represented by the following formula 3.
[0070] [Chemical formula 3]
[0071]
[0072] R in the formula 4 is a hydrogen atom or a methyl group. 5 It is an organic group having 2 to 20 carbon atoms.
[0073] R in the formula 4is a hydrogen atom or a methyl group, and a hydrogen atom is preferred from the viewpoint of increasing the flexibility of the cured product of the curable resin composition and improving the impact resistance of the sealing material. 5 The number of carbon atoms in is preferably 2 to 15, more preferably 5 to 15. 5 When the number of carbon atoms is within this range, the usability of the curable resin composition in an uncured state can be improved while maintaining the flexibility of the cured product of the curable resin composition and the high impact resistance of the sealing material.
[0074] The organic group refers to a group containing C and further containing at least one element selected from the group consisting of Si, N, P, O and S. The organic group may also be a polymer having a repeating unit. In addition, in its structure, groups such as ketone groups, ester groups, ether groups, thioether groups, isocyanurate groups, etc. may also be contained.
[0075] Specific examples thereof include (meth)allyl methyl ether, (meth)allyl ethyl ether, (meth)allyl butyl ether, (meth)allyl octyl ether, (meth)allyl benzyl ether, phenyl (meth)allyl ether, (meth)allyl methyl sulfide, (meth)allyl cyclohexane, (meth)allyl acetate, (meth)allyl hexanoate, (meth)allyloxytetrahydrofuran, (meth)allyl glycidyl ether, and 1-(meth)allyl-3,5-diglycidyl isocyanurate.
[0076] Among the above (meth)allyl compounds, 1-allyl-3,5-diglycidyl isocyanurate is preferred from the viewpoints of preventing the sealing material from being discolored over time, increasing the flexibility of the cured product of the curable resin composition, and improving the impact resistance of the sealing material.
[0077] The molecular weight of the monofunctional (meth)allyl compound (D) is preferably 200 to 1,000 from the viewpoint that the curable resin composition has excellent usability in an uncured state and the impact resistance of the sealing material can be improved.
[0078] <Photopolymerization initiator (E)>
[0079] Photopolymerization initiator (E) is a component added to promote the curing reaction of the polymerizable compound by light when adding the above-mentioned (A), the above-mentioned (B), the above-mentioned (C), the above-mentioned (D) and other polymerizable compounds, and it can reduce the light required for the curing of the curable resin composition. Photopolymerization initiator (E) can be used alone or in combination of two or more. As the photopolymerization initiator, photoradical polymerization initiator, photocationic polymerization initiator, photoanionic polymerization initiator, etc. can be listed. Among them, from the perspective of shortening the reaction time and improving productivity, photoradical polymerization initiator is preferred.
[0080] Examples of the photoradical polymerization initiator include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propynyl)-benzyl]-phenyl}-2-methyl-propane-1-one, 1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(o-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone-1-(o-acetyl oxime), etc.
[0081] Examples of the photocationic polymerization initiator include bis(4-tert-butylphenyl)iodonium hexafluorophosphate, bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, cyclopropyldiphenylsulfonium tetrafluoroborate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroarsenate, 2-(3,4-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, triphenylsulfonium tetrafluoroborate, triphenylsulfonium bromide, tri-p-tolylsulfonium hexafluorophosphate, and tri-p-tolylsulfonium trifluoromethanesulfonate.
[0082] Examples of the photoanionic polymerization initiator include acetophenone O-benzoyl oxime, nifedipine, 2-(9-oxoxanthen-2-yl)propionic acid, 1,5,7-triazidobicyclo[4,4,0]dec-5-ene, 2-nitrophenylmethyl 4-methacryloyloxypiperidine-1-carboxylate, 2-(3-benzoylphenyl)propionic acid 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidine, and 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidine n-butyltriphenylborate.
[0083] <Spherical filler (F)>
[0084] The curable resin composition of the present invention may also contain a spherical filler (F) within the range that does not hinder the purpose of the present invention. The spherical filler (F) preferably has an average particle size of less than 15 μm, and more preferably has an average particle size of less than 10 μm. If the average particle size is within this range, the flexibility and toughness of the curable resin composition will not be impaired, and the adhesion and impact resistance of the sealing material to the curved film substrate can be maintained. In addition, the average particle size can be measured using a commercially available particle size distribution measuring device such as MicrotracMT-3000II manufactured by MicrotracBEL Corp.
[0085] As the spherical filler (F) composed of an inorganic substance, for example, there can be mentioned silicon dioxide, silicon carbide, calcium carbonate, magnesium carbonate, aluminum oxide, titanium dioxide, calcium oxide, magnesium oxide, magnesium hydroxide, aluminum hydroxide, etc. Among them, silicon dioxide is preferred from the viewpoints of not impairing the water barrier property of the sealing material, maintaining the performance of suppressing orientation disorder even when exposed to a severe wet heat test, and improving the shape stability.
[0086] Examples of the spherical filler (F) composed of an organic substance include acrylic particles, urethane particles, styrene particles, melamine particles, acrylic-styrene particles, etc. Among them, acrylic particles and urethane particles are preferred because they do not impair the flexibility and toughness of the curable resin composition and can maintain the adhesion and impact resistance of the sealing material to the curved film substrate.
[0087] These spherical fillers may be used alone or in combination of two or more.
[0088] The true density of the spherical filler (F) is preferably 1.1 to 4.0, more preferably 1.2 to 3.0, from the viewpoint of not impairing the flexibility and toughness of the curable resin composition and being able to maintain the adhesion and impact resistance of the sealing material to the curved film substrate. In addition, the true density can be measured by using a commercially available specific gravity meter (pycnometer) such as Ultrapyc1200e manufactured by Quantachrome Instruments Japan Joint Venture.
[0089] The content of the spherical filler (F) in the curable resin composition of the present invention is preferably 0.5 to 50 parts by mass, more preferably 1 to 40 parts by mass, based on 100 parts by mass in total of (A), (B), (C) and (D).
[0090] <Other ingredients>
[0091] The curable resin composition of the present invention may further contain additives such as (meth)acrylic compounds, epoxy compounds and other polymerizable compounds, surfactants, silane coupling agents, curing accelerators, ultraviolet absorbers, light stabilizers, antioxidants, polymerization inhibitors, leveling agents, adhesion promoters, plasticizers, defoaming agents, light-shielding materials, conductive materials, spacers, and shape stabilizing materials, within a range that does not impair the purpose of the present invention.
[0092] <Composition ratio (blending ratio)>
[0093] The curable resin composition of the present invention can obtain a cured product by a thiol-ene reaction between the thiol group of a multifunctional thiol compound (A) and the polymerizable unsaturated bonds of a multifunctional urethane (meth)acrylate compound (B), a multifunctional (meth)allyl compound (C) and a monofunctional (meth)allyl compound (D), wherein the blending mass ratio (B) / [(C)+(D)] of (B) to (C) and (D) is 0.1 to 1.0, the blending mass ratio (C) to (D) is 0.3 to 3.0, and the functional group concentration of the thiol group of (A) is 1.0 to 1.0. The curable resin composition (B), (C) and (D) are blended in such a manner that the total ratio of the functional group concentration of the polymerizable unsaturated bond (thiol group / polymerizable unsaturated bond) is 0.4 to 3.0. The curable resin composition has excellent usability in an uncured state and does not contaminate the liquid crystal even when it comes into contact with the liquid crystal. The sealing material composed of the cured product of the curable resin composition does not cause orientation disorder of the liquid crystal even when it comes into contact with the liquid crystal in a harsh hot and humid environment, has excellent adhesion to a curved film substrate, and further has high impact resistance that does not peel off from the film substrate even when an impact is applied. The functional group concentration of thiol groups is a number represented by the total of 100 parts by mass of (A) among (A), (B), (C) and (D) × the number of functional groups of thiol groups in (A) / the molecular weight of (A), and the total functional group concentration of polymerizable unsaturated bonds of (B) and (C) is a number represented by [the total of 100 parts by mass of (B) among (A), (B), (C) and (D) × the number of (meth)acryloyl groups in (B) / the molecular weight of (B)] + [the total of 100 parts by mass of (C) among (A), (B), (C) and (D) × the number of allyl groups in (C) / the molecular weight of (C)] + [the total of 100 parts by mass of (D) among (A), (B), (C) and (D) × the number of allyl groups in (D) / the molecular weight of (D)]. Therefore, the curable resin composition of the present invention cannot lack any one of (A), (B), (C) and (D). In addition, by further using the above-mentioned (E) in the curable resin composition containing (A), (B), (C) and (D), it is possible to cure only by light irradiation and show the above-mentioned effect. In addition, due to the presence of (B) which has high polarity and is easy to interact strongly via hydrogen bonds, the curable resin composition has strong drawing properties in the uncured state, resulting in reduced usability, but the curable resin composition of the present invention can reduce the drawing properties by containing (D), thereby ensuring usability.
[0094] In the curable resin composition of the present invention, in order to improve the non-liquid crystal contamination, even if it comes into contact with the liquid crystal in the uncured state, the liquid crystal will not be contaminated, and the toughness of the cured product of the curable resin composition and the adhesion to the substrate are improved, and the adhesion and impact resistance of the sealing material to the curved film substrate are improved. It is preferred that in a total of 100 parts by mass of (A), (B), (C) and (D), more than 5 parts by mass of (B) are contained, and more preferably more than 10 parts by mass of (B) are contained. In addition, in order to reduce the stringiness of the curable resin composition, and in order to make the usability in the uncured state excellent, and to improve the water barrier of the cured product of the curable resin composition, and to suppress the orientation disorder of the sealing material under the harsh wet heat test, it is preferred that in a total of 100 parts by mass of (A), (B), (C) and (D), less than 35 parts by mass of (B) are contained, and more preferably less than 20 parts by mass of (B) are contained. That is, in order to simultaneously achieve at a higher level the following properties: the curable resin composition has excellent usability in an uncured state, does not contaminate the liquid crystal even when in contact with the liquid crystal, suppresses the orientation disorder of the liquid crystal even when the sealing material is exposed to a severe heat and humidity test, has excellent adhesion to a curved film substrate, and has various properties of high impact resistance, it is preferred that in a total of 100 parts by mass of (A), (B), (C) and (D), the amount of (B) is not less than 5 parts by mass and not more than 35 parts by mass, and it is more preferred that the amount of (B) is not less than 10 parts by mass and not more than 20 parts by mass.
[0095] In addition, in the curable resin composition of the present invention, in order to suppress the degree of viscosity increase and stringiness and to improve the usability in the uncured state, the blending mass ratio (B) to (C) and (D) (B) / [(C)+(D)] is preferably 0.2 to 0.7; in order to improve the water barrier properties of the cured product of the curable resin composition and further suppress the orientation disorder of the sealing material under the harsh wet heat test, the blending mass ratio (B) to (C) and (D) (B) / [(C)+(D)] is preferably 0.6 or less; in order to improve the toughness of the cured product of the curable resin composition and to improve the adhesion of the sealing material to a curved film substrate, the blending mass ratio (B) to (C) and (D) is preferably 0.6 or less. ) / [(C)+(D)] is preferably 0.2 or more; in order to improve the flexibility of the cured product of the curable resin composition and further improve the impact resistance of the sealing material, the blending mass ratio of (B) to (C) and (D) (B) / [(C)+(D)] is preferably 0.3 or more, that is, in order to simultaneously achieve various properties at a higher level, including excellent usability of the curable resin composition in an uncured state, suppression of liquid crystal orientation disorder even when the sealing material is exposed to a harsh wet heat test, excellent adhesion of the sealing material to a curved film substrate, and high impact resistance of the sealing material, the blending mass ratio of (B) to (C) and (D) (B) / [(C)+(D)] is preferably 0.3~0.6.
[0096] Furthermore, in the curable resin composition of the present invention, in order to further suppress the degree of viscosity increase and stringiness in the uncured state and improve the usability, the blending mass ratio (C) / (D) is preferably 2.6 or less; in order to improve the water barrier properties of the cured product of the curable resin composition, further suppress the orientation disorder of the sealing material under the harsh wet heat test, and improve the toughness of the cured product of the curable resin composition, so that the adhesion to a more curved film substrate is excellent, the blending mass ratio (C) / (D) is preferably 0.5 or more; In order to improve the flexibility of the cured product of the curable resin composition and further improve the impact resistance of the sealing material, the blending mass ratio (C) to (D) (C) / (D) is preferably 2.4 or less. That is, in order to simultaneously achieve at a higher level the excellent usability of the curable resin composition in an uncured state, the various properties of suppressing the orientation disorder of the liquid crystal even when the sealing material is exposed to a severe wet heat test, the excellent adhesion of the sealing material to a curved film substrate, and the high impact resistance of the sealing material, the blending mass ratio (C) to (D) (C) / (D) is preferably 0.5 to 2.4.
[0097] In addition, in the curable resin composition of the present invention, in order to improve the water barrier properties of the cured product of the curable resin composition and further suppress the orientation disorder of the sealing material under the harsh wet heat test, the ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bond of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is preferably 0.7 to 2.3; in order to improve the toughness of the cured product of the curable resin composition and make the adhesion to the curved film substrate excellent, the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bond of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is preferably 0.7 to 2.5 ... is preferably 0.7 to 2.5. In order to improve the flexibility of the cured product of the chemical resin composition and further improve the impact resistance of the sealing material, the ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bonds of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is preferably 0.7 or more. That is, in order to simultaneously achieve various properties at a higher level, such as suppression of orientation disorder of liquid crystal even when the sealing material is exposed to a severe wet heat test, excellent adhesion of the sealing material to a curved film substrate, and high impact resistance of the sealing material, the ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bonds of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is preferably 0.7 to 2.3.
[0098] Furthermore, in the curable resin composition of the present invention, the ratio of (E) to a total of 100 parts by mass of (A), (B), (C) and (D) is preferably 0.01 to 10.0 parts by mass, and more preferably 0.1 to 10.0 parts by mass. By making the content of (E) within the above range, a sealing material can be obtained which does not cause orientation disorder of the liquid crystal even when in contact with the liquid crystal under a harsh hot and humid environment, has excellent adhesion to a curved film substrate, and has high impact resistance.
[0099] <Film LCD Panel>
[0100] The film liquid crystal panel of the present invention includes: for example, a dimming component that uses the orientation of liquid crystal to control only transparency / opaqueness or a display element that displays images like a display. The film liquid crystal panel of the present invention is, for example, a structure in which a pair of substrates are arranged relative to each other and sealed on all sides with the above-mentioned film liquid crystal panel sealing material, and a liquid crystal material exists between them. Here, the substrate refers to a structure in which a silver or copper electrode or a transparent electrode such as ITO, PEDOT is applied to a plastic transparent film substrate such as polyethylene terephthalate, polycarbonate, cycloolefin (co)polymer, PMMA, polyimide, etc. In addition, it also includes a structure in which an orientation film is further formed on the transparent electrode.
[0101] The film liquid crystal panel of the present invention is a liquid crystal panel formed on a substrate using the above-mentioned plastic transparent film base material, and the sealing material for a film liquid crystal panel is a sealing material used for the above-mentioned film liquid crystal panel.
[0102] <Formation of film liquid crystal panel>
[0103] The film liquid crystal panel of the present invention can be formed by coating the curable resin composition of the present invention on one of the pair of substrates, dripping liquid crystal on the inner side thereof, superimposing the other substrate, and irradiating light to cure the curable resin composition. In addition, it can also be formed by coating a polymer-dispersed liquid crystal containing liquid crystal and a curable resin composition on one of the pair of substrates, superimposing the other substrate, irradiating light to cure the polymer-dispersed liquid crystal, and then coating the curable resin composition of the present invention on the periphery thereof, irradiating light to cure the curable resin composition.
[0104] The method for applying the curable resin composition is not particularly limited, and for example, a method using a coating device such as a dispenser, an inkjet method, or a screen printing method, or a method of manual application using a syringe or a brush, etc. can be appropriately used.
[0105] There is no particular limitation on the light source for irradiating the curable resin composition. For example, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a black light lamp, an LED lamp, a halogen lamp, an electrodeless lamp, a xenon lamp, a mercury fluorescent lamp, an LED fluorescent lamp, sunlight, an electron beam irradiation device, etc. can be appropriately used.
[0106] Regarding the contamination of the film liquid crystal panel, in addition to forming the film liquid crystal panel in the above manner and actually applying voltage to confirm the orientation, it can also be evaluated by measuring the voltage holding rate. The voltage holding rate is an evaluation method for confirming the extent to which the charge charged by applying voltage to the liquid crystal box is maintained after a certain period of time. When the liquid crystal is contaminated, the charge cannot be maintained, resulting in a decrease in the voltage holding rate. A good voltage holding rate without contamination is 90% or more, preferably 95% or more.
[0107] Example
[0108] Next, the present invention will be described in further detail with reference to Examples and Comparative Examples.
[0109] <Evaluation Method>
[0110] The curable resin compositions in the respective Examples and Comparative Examples were evaluated for performance by the following methods.
[0111] <Usability of curable resin composition>
[0112] The curable resin composition manufactured in the embodiment and the comparative example is filled into a UV shielding syringe (PSY-20FU-OR manufactured by Musashi Engineering, Inc.) that can shield visible light, and is left to stand in a room at 25°C for 5 days. Then, the syringe is set on a dispensing machine (SHOTMASTER manufactured by Musashi Engineering, Inc.), and the dispensing machine is used to coat 3 circular shapes with a diameter of 2 mm at intervals of 1 cm in 9 seconds (3 seconds per point) on a 40mm×45mm glass substrate (RT-DM88-PIN manufactured by EHC.Co., Ltd.) on which a transparent electrode and an oriented film are sequentially arranged on the glass, and the coated points are observed with the naked eye. In addition, the more coating can be performed, and further, the more it can be coated without shrinking or oozing out of a circular shape with a diameter of 2 mmΦ, the higher the usability, and the results are recorded in each table.
[0113] ◎: The curable resin composition can be applied, and all three points can be applied in a circular shape with a diameter of 2 mm without shrinking or bleeding of the curable resin composition;
[0114] ○: Although the curable resin composition can be applied, shrinkage or bleeding from a circular shape with a diameter of 2 mm is observed at any one of the three points;
[0115] ×: The curable resin composition gelled in the syringe and could not be applied.
[0116] <Non-liquid crystal contamination>
[0117] 0.025 g of the curable resin composition was added to a sample bottle, and 1 g of liquid crystal (MLC-7021-000 manufactured by Merck) was further added, and the mixture was left to stand at 25° C. for 1 hour. Then, ultraviolet irradiation (1000 mJ / cm 2 ), the curable resin composition was cured and heated at 100°C for 2 hours. After 2 hours, the cured product and the liquid crystal were separated by a centrifugal separator, and the liquid crystal was injected into a glass substrate liquid crystal box with ITO (KSSZ-05 / B107MINX05 manufactured by EHC.Co., Ltd.). Using a liquid crystal property evaluation system (6245 manufactured by TOYO Corporation), an initial voltage of 5V AC for 64μs was applied to the liquid crystal box at 25°C, and the value (voltage holding ratio) obtained by multiplying the voltage ratio before and after the frame generation time (frame time) of 16.7ms by 100 was calculated. In addition, the higher the voltage holding ratio, the more difficult it is for the liquid crystal to be contaminated, and the voltage holding ratio is recorded as non-liquid crystal contamination in each table.
[0118] <Orientation disorder in harsh hot and humid environments>
[0119] Using a dispensing machine (SHOTMASTER manufactured by Musashi Engineering, Inc.), the curable resin composition manufactured in the embodiment and the comparative example was applied into a 35mm×40mm quadrilateral frame (line width: 1mm) on a 40mm×45mm glass substrate (RT-DM88-PIN manufactured by EHC.Co., Ltd.) on which a transparent electrode and an orientation film were sequentially arranged on the glass, and liquid crystal (MLC-11900-000 manufactured by Merck) was dripped into the inner side of the curable resin composition drawn on the frame. Then, the above-mentioned glass substrate and the opposite glass substrate were bonded to each other under reduced pressure and left to stand at 25°C for 1 hour. Ultraviolet irradiation was performed using a high-pressure mercury lamp (1000mJ / cm 2), a liquid crystal panel was obtained. After the liquid crystal panel prepared in the same manner as above was exposed to 60°C and 90%RH for 1000 hours, it was driven at a voltage of AC5V and in a mid-tone display state, and the orientation disorder of the liquid crystal near the sealing material composed of the cured product of the curable resin composition was observed by a polarizing microscope. In addition, the shorter the distance over which the orientation disorder diffuses from the end of the sealing material, the more difficult it is for the orientation disorder to occur, and the distance over which the orientation disorder diffuses is recorded in each table.
[0120] ◎: Orientation disorder starts from the end of the sealing material and does not spread beyond 0.3 mm;
[0121] ○: The orientation disorder starts to spread from the end of the sealing material to more than 0.3 mm, but does not spread to more than 0.6 mm;
[0122] ×: Orientation disorder spreads from the edge of the sealing material to exceed 0.6 mm.
[0123] <Adhesion>
[0124] Two ITO films (TETOLIGHT TCF manufactured by OIKE & Co., Ltd., with a thickness of 125 μm) were prepared. The curable resin composition prepared in the examples and comparative examples was applied to the ITO surface of one ITO film using an applicator, and the other ITO film was laminated so that its ITO surface was in contact with the curable resin composition. Ultraviolet irradiation (1000 mJ / cm 2 ), obtain the sample (thickness of cured film: 100 μm) formed by clamping cured film with ITO film. It is cut into a rectangular shape of 150 mm long and 25 mm wide, and used as an evaluation sample. The obtained sample is set on a universal testing machine (Autograph) (universal testing machine AG-IS manufactured by SHIMADZU CORPORATION), and a T-type peeling test is carried out according to JISK 6854-3 to evaluate adhesion (tensile speed: 10 mm / minute). In addition, the larger the value, the higher the adhesion, and the result is recorded in each table.
[0125] ◎: 8.0N / 25mm or more
[0126] ○: 4.0N / 25mm or more and less than 8.0N / 25mm
[0127] ×: less than 4.0N / 25mm
[0128] <Impact resistance>
[0129] The evaluation sample prepared in the same manner as the above-mentioned adhesion evaluation was placed on a rubber plate with a thickness of 10 cm, and a metal ball with a diameter of 38 mm and a mass of 230 g was dropped from a height of 10 cm or 20 cm onto the evaluation sample. The position impacted by the metal ball was observed with the naked eye to confirm whether floating or peeling occurred. In addition, the higher the height until floating or peeling occurred, the better the impact resistance, and the results were recorded in each table.
[0130] ⊚: No floating or peeling occurred even when the metal ball was dropped from a height of 20 cm.
[0131] ○: Although no floating or peeling occurred when the metal ball was dropped from a height of 10 cm, floating or peeling occurred when the metal ball was dropped from a height of 20 cm.
[0132] ×: The metal ball dropped from a height of 10 cm caused the product to float or peel off.
[0133] <Multifunctional thiol compound (A)>
[0134] A-1: Dipentaerythritol hexa(3-mercaptopropionate) [Number of thiol groups: 6]
[0135] A-2: Pentaerythritol tetrakis(3-mercaptopropionate) [Number of thiol groups: 4]
[0136] A-3: Tris-[(3-mercaptopropyleneoxy)-ethyl]-isocyanurate [Number of thiol groups: 3]
[0137] <Synthesis of polyfunctional urethane (meth)acrylate (B)>
[0138] [Synthesis of polyol compound (b-1)]
[0139] 151.5 parts by mass of pimelic acid and 187.3 parts by mass of diethylene glycol were added to a reaction vessel equipped with a stirrer, a distillation tower, a nitrogen inlet pipe, and a thermometer, and heated to 140°C under a nitrogen atmosphere and stirred. 0.01 parts by mass of tetrabutyl titanate was added thereto and the temperature was raised to 220°C to carry out a dehydration reaction. Then, the temperature was maintained at 220°C to carry out the dehydration reaction. 18 hours after the start of the dehydration reaction, the contents were cooled to obtain a diol compound (b-1) (weight average molecular weight: 1,000).
[0140] [Synthesis of polyol compound (b-2)]
[0141] 150.2 parts by mass of adipic acid and 158.3 parts by mass of 3-methyl-1,5-pentanediol were added to a reaction vessel equipped with a stirrer, a distillation tower, a nitrogen inlet pipe, and a thermometer, and heated to 140°C and stirred under a nitrogen atmosphere. 0.01 parts by mass of tetrabutyl titanate was added thereto and the temperature was raised to 220°C for dehydration reaction. Then, the temperature was kept at 220°C for dehydration reaction. 18 hours after the dehydration reaction started, the contents were cooled to obtain a diol compound (b-2) (weight average molecular weight: 1,500).
[0142] [Synthesis of polyol compound (b-3)]
[0143] 160.3 parts by mass of diphenyl carbonate, 234.1 parts by mass of 1,6-hexanediol, and 0.1 parts by mass of tetrabutyl titanate were added to a reaction vessel equipped with a stirrer, a fractionator, an air condenser, a thermometer, a receiver, and a vacuum device, and heated to 100° C. under a reduced pressure of 10 Torr and stirred for 5 hours. Phenol as a by-product was distilled off, and the contents were cooled to obtain a diol compound (b-3) (weight average molecular weight: 600).
[0144] [Synthesis of urethane (meth)acrylate (B-1)]
[0145] 101.1 parts by mass of the polyol compound (b-1) was added to a reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer, and stirring was started. Next, 0.1 parts by mass of dibutyltin laurate and 32.1 parts by mass of isophorone diisocyanate as a diisocyanate were added, and the internal temperature was raised to 80°C while paying attention to heat generation, and then the temperature was maintained and stirred for 3 hours. Furthermore, 0.1 parts by mass of p-hydroxyanisole as a polymerization inhibitor and 24.0 parts by mass of 2-hydroxyethyl acrylate as a (meth)acrylate having a hydroxyl group were added, and stirred at 85°C for 2 hours to obtain urethane (meth)acrylate (B-1) (weight average molecular weight: 3000).
[0146] [Synthesis of (B-2) to (B-5)]
[0147] Polyfunctional urethane (meth)acrylates (B-2) to (B-5) were obtained in the same manner as above except that the polyol compound, diisocyanate compound and (meth)acrylate compound having a hydroxyl group in Table 1 were used.
[0148] [Table 1]
[0149]
[0150] <Polyfunctional (meth)allyl compound (C)>
[0151] C-1: 1,3-diallyl-5-glycidyl isocyanurate [number of allyl groups: 2]
[0152] C-2: Triallyl isocyanurate [Number of allyl groups: 3]
[0153] C-3: Pentaerythritol tetraallyl ether [Number of allyl groups: 4]
[0154] <Monofunctional (meth)allyl compound (D)>
[0155] D-1: 1-allyl-3,5-diglycidyl isocyanurate [molecular weight: 281.3]
[0156] D-2: Butyl allyl ether [Molecular weight: 114.2]
[0157] D-3: Allyl glycidyl ether [Molecular weight: 114.1]
[0158] <Monofunctional (meth)acrylic compound (D')>
[0159] D'-1: Lauryl Methacrylate
[0160] <Photopolymerization initiator (E)>
[0161] E-1: Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide
[0162] E-2: 1-Hydroxycyclohexyl phenyl ketone
[0163] E-3: 2,4,6-Trimethylbenzoyl-diphenyl-phosphine oxide
[0164] <Spherical filler (F)>
[0165] F-1: AEROSIL RX-200 [average particle size: 12nm, true density: 2.2g / cm 3 ] Silica particles manufactured by NIPPON AEROSIL CO.,LTD.
[0166] F-2: SE-010T [average particle size: 10 μm, true density: 1.2 g / cm 3 ] Acrylic particles manufactured by Negami Chemical Industrial Co., Ltd.
[0167] F-3: C-400T [average particle size: 15 μm, true density: 1.2 g / cm 3 ] Urethane granules manufactured by Negami Chemical Industrial Co., Ltd.
[0168] [Examples 1 to 36 and Comparative Examples 1 to 13]
[0169] The above components were added to a planetary mixer in the amounts shown in Tables 2 and 3 below, and mixed and stirred for 2 hours to obtain a curable resin composition. The curable resin composition was used to perform various evaluations. The results are shown in Tables 2-1, 2-2, 2-3, 3-1, and 3-2.
[0170] [Table 2-1]
[0171]
[0172] [Table 2-2]
[0173]
[0174] [Table 2-3]
[0175]
[0176] [Table 3-1]
[0177]
[0178] [Table 3-2]
[0179]
[0180] According to the above test results, the curable resin composition of each embodiment contains the components (A) to (E) in appropriate amounts as specified in the present invention, and has excellent usability and non-liquid crystal contamination properties. After curing, it will not cause orientation disorder of the liquid crystal even in a harsh hot and humid environment, and has excellent adhesion to the film substrate and further has high impact resistance.
[0181] However, for Comparative Example 1, since it does not contain the multifunctional thiol compound (A), the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under the harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low. For Comparative Example 2, since it does not contain the multifunctional urethane (meth) acrylate compound (B), the non-liquid crystal contamination of the curable resin composition is poor, and the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under the harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low. For Comparative Example 3, since it does not contain the multifunctional (meth) allyl compound (C), the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under the harsh wet heat test, and the adhesion to the film substrate is also low. For Comparative Example 4, since it does not contain a monofunctional (meth)allyl compound (D), the usability of the curable resin composition is poor, and the impact resistance of the film liquid crystal panel sealing material obtained by curing the curable resin composition is low. For Comparative Example 5, since it does not contain a photopolymerization initiator (E), the film liquid crystal panel sealing material obtained by curing the curable resin composition causes orientation disorder of the liquid crystal under a harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low.
[0182] For Comparative Example 6, since the blending mass ratio (B) / [(C)+(D)] is smaller than the prescribed range, the non-liquid crystal contamination of the curable resin composition is poor, and the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under a harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low. For Comparative Example 7, since the blending mass ratio (B) / [(C)+(D)] is larger than the prescribed range, the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under a harsh wet heat test.
[0183] For Comparative Example 8, since the blending mass ratio (C) / (D) is smaller than the prescribed range, the film liquid crystal panel sealing material obtained by curing the curable resin composition causes orientation disorder of the liquid crystal under a harsh wet heat test, and the adhesion to the film substrate is also low. For Comparative Example 9, since the blending mass ratio (C) / (D) is larger than the prescribed range, the usability of the curable resin composition is poor, and the impact resistance of the film liquid crystal panel sealing material obtained by curing the curable resin composition is low.
[0184] For Comparative Example 10, since the ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bonds of (B), (C) and (D) is smaller than the prescribed range, the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under the harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low. For Comparative Example 11, since the ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bonds of (B), (C) and (D) is larger than the prescribed range, the film liquid crystal panel sealing material obtained by curing the curable resin composition causes the orientation disorder of the liquid crystal under the harsh wet heat test, and the adhesion and impact resistance to the film substrate are also low.
[0185] For Comparative Examples 12 and 13, since a monofunctional (meth)acrylic compound is used instead of a monofunctional (meth)allyl compound (D), the impact resistance of the sealing material for a film liquid crystal panel obtained by curing the curable resin composition is low. In addition, for Comparative Example 12, it causes orientation disorder of the liquid crystal under a harsh wet heat test and has low adhesion to the film substrate.
Claims
1. A curable resin composition for a film liquid crystal panel sealing material, comprising: (A) a multifunctional thiol compound having 2 to 6 thiol groups, (B) a polyfunctional urethane (meth)acrylate compound having 2 to 3 (meth)acryloyl groups, (C) a polyfunctional (meth)allyl compound having 2 to 4 (meth)allyl groups, (D) a monofunctional (meth)allyl compound having one (meth)allyl group, and (E) a photopolymerization initiator, The blending mass ratio of (B) to (C) and (D) is (B) / [(C)+(D)] 0.1~1.0, The blending mass ratio of (C) to (D) is (C) / (D) in the range of 0.3 to 3.
0. The ratio of the functional group concentration of the thiol group of (A) to the total functional group concentration of the polymerizable unsaturated bond of (B), (C) and (D) (thiol group / polymerizable unsaturated bond) is 0.4 to 3.
0.
2. A film liquid crystal panel, wherein: The end is sealed with the curable resin composition according to claim 1.
Citation Information
Patent Citations
Sealant for display elements
JP2016169298A
Display element sealing agent
JP2017054084A
Curable resin composition used in sealing material for film liquid crystal panel, and film liquid crystal panel with sealed end with the curable resin composition
JP2021162680A
Cited By
UV (ultraviolet) light-cured resin composition as well as preparation method and application thereof
CN119505239A