Precious metal high-dispersion VOCs catalytic oxidation catalyst as well as preparation method and application thereof
By controlling the pH value of the precious metal nitrate hydrolysis process and combining oxygen storage materials, a high-active catalyst layer was prepared, which solved the problem of limited loading of precious metals in the catalyst and achieved efficient VOCs oxidation effect.
Patent Information
- Application Number
- CN202310597244.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-29
AI Technical Summary
The loading of precious metals in existing catalytic oxidation catalysts is limited, which makes it difficult to further improve the performance of the catalyst. How to improve the utilization efficiency of precious metals under the premise of low active component loading is an urgent problem.
Using precious metal nitrate as the precursor, the pH value of the hydrolysis process is controlled by buffer reagents to form precious metal particles with high dispersion. Combining oxygen storage materials and binders, a catalyst layer with high activity is prepared, which increases the low temperature of the catalyst. Catalytic oxidation properties.
It is achieved to improve the VOCs oxidation activity of the catalyst under low noble metal loading, reduce the conversion temperature, improve the reaction efficiency, is suitable for mass production, and significantly improve the dispersion of precious metals on the support surface.
Smart Images

Figure BDA0004247587190000091 
Figure HDA0004247587200000011 
Figure HDA0004247587200000012
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst preparation, and in particular to a VOCs catalytic oxidation catalyst and a preparation method thereof, and application of the catalyst in catalytic oxidation of VOCs. Background Art
[0002] Volatile Organic Compounds (VOCs) are the main pollutants in waste gas emitted during the production and processing of various industries such as petrochemicals, printing, and pharmaceuticals. They have a noticeable odor and can irritate or harm human organs. In severe cases, they can cause poisoning or cancer, endangering human health. In addition, VOCs participate in the formation of ozone and secondary aerosols in the atmospheric environment, and have an important impact on regional atmospheric ozone pollution and PM2.5 pollution.
[0003] VOCs pollution control can be divided into adsorption, incineration, catalytic oxidation, biological methods and membrane separation methods. Among them, catalytic oxidation technology is one of the most promising technologies for removing VOCs; and the development of high-performance catalytic oxidation catalysts is the key to achieving exhaust gas purification and green production. At present, catalytic oxidation catalysts are mostly based on honeycomb inert materials (such as cordierite, etc.) as carriers, loaded with active components with low-temperature oxidation properties to achieve VOCs catalytic oxidation.
[0004] VOCs oxidation catalysts usually use precious metals such as platinum and palladium as active components. These precious metals can activate hydrocarbons and oxygen at low temperatures, allowing the two to react on their surfaces via the LH mechanism, thus exhibiting excellent low-temperature catalytic oxidation activity.
[0005] However, the high price of precious metals determines that the precious metal loading in oxidation catalysts is limited (usually less than 2%), making it difficult to further improve the performance of the catalyst. How to improve the efficiency of precious metal utilization by improving slurry preparation technology under the premise of low active component loading is an urgent problem to be solved in this field. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a VOCs low-temperature catalytic oxidation catalyst with low active component loading and high activity, wherein the noble metal loading of the catalyst is less than 2g / L carrier. The second technical problem to be solved by the present invention is to provide a method for preparing the catalyst.
[0007] The present invention provides a VOCs catalytic oxidation catalyst, which comprises a carrier and a catalyst layer loaded on the carrier, wherein the catalyst layer comprises a matrix material loaded with active components, an oxygen storage material, zirconium oxide and a binder oxide, and the matrix material loaded with the active components comprises a noble metal, an alkaline earth metal and / or an alkali metal, and a matrix; and the average particle size of the noble metal in the matrix material loaded with the active components is 1.4-2.4 nm.
[0008] The second aspect of the present invention provides a method for preparing a VOCs catalytic oxidation catalyst, the method comprising:
[0009] (1) mixing a buffer agent, an alkali metal and / or alkaline earth metal salt, an optional oxygen storage material, a matrix source and water, and then adding a noble metal nitrate to form a mixed solution, referred to as a first mixed solution, slowly hydrolyzing the noble metal ions under ultrasonic stirring and the pH value of the buffer solution, drying and ozone roasting to obtain an active component-loaded matrix material; the mass concentration of the buffer agent in the first mixed solution is preferably 0.5%-5%; the pH value of the buffer solution is 1.5-3.5, preferably 1.5-3;
[0010] (2) mixing the matrix material loaded with the active component, the optional oxygen storage material, zirconium acetate, the binder oxide and water to obtain a second mixed solution, and grinding the mixed solution to obtain a catalyst slurry; the grinding may be performed by ball milling; wherein the oxygen storage material is added in step (1) and / or step (2), and preferably, all of the oxygen storage material is added in step (2);
[0011] (3) The catalyst slurry is loaded onto a carrier, and after drying and calcination, a VOCs catalytic oxidation catalyst loaded with a catalyst layer is obtained.
[0012] In the existing methods for preparing VOCs oxidation catalysts containing precious metals, the introduction of precious metals usually adopts metal nitrates, chlorides or chlorates of precious metals, and organic salts of precious metals. The inventors of the present application have found that when using precious metal nitrates, nitrate ions decompose during the roasting process to form precious metal elements or oxides, and no anions remain, but the dispersion of the precious metals in the obtained VOCs oxidation catalyst is not high. In contrast, although precious metal chlorides or chlorates partially decompose to generate chlorine and hydrogen chloride during the roasting process, it is inevitable that a small amount of chloride ions remain in the catalyst coating, causing poisoning of the precious metal active center during use. Precious metal organic salts (common such as acetates and propionates) need to be used in conjunction with toxic organic solvents such as acetone and toluene to avoid hydrolysis. Because the regular catalyst coating workshop usually adopts an open design, organic salts are not suitable for large-scale industrial production.
[0013] After research, the inventors of the present application believe that the nitric acid concentration in the precious metal nitrate solution used in industry is high (pH value is less than 1). When the precious metal nitrate solution is added to the slurry, the pH of the slurry drops rapidly to below 1.5, at which time the precious metal cations have not yet been hydrolyzed (precious metal cations such as platinum and palladium begin to hydrolyze at a pH above 1.5); subsequently, the nitrate ions react with the surface hydroxyl groups of the oxide (mainly the matrix material such as the alumina matrix material) in the slurry by acid-base reaction, and the pH of the slurry rises rapidly. As the pH increases, the hydroxide concentration in the solution increases, the hydrolysis rate of the precious metal accelerates, and the hydroxide precursor particles formed are larger in size.
[0014] In the present invention, an organic acid is used as a buffering agent. After the strong acid (nitric acid) is consumed by the surface hydroxyl groups of the oxide, the organic acid reacts with the surface hydroxyl groups to form a buffering system, which plays a role in accurately controlling the pH value of the hydrolysis process and reducing the hydrolysis rate of the noble metal nitrate, thereby inhibiting the growth of the noble metal hydroxide precursor particles formed by hydrolysis.
[0015] The third aspect of the present invention provides a catalyst prepared according to the method described above.
[0016] The fourth aspect of the present invention is to use the VOCs oxidation catalyst as described above in catalytic oxidation of VOCs. Specifically, the present invention provides a VOCs catalytic oxidation method, comprising contacting a gas containing VOCs and oxygen with the VOCs catalytic oxidation catalyst provided by the present invention, wherein the VOCs include, for example, one or more of propylene, propane, benzene, and toluene.
[0017] The VOCs catalytic oxidation catalyst provided by the present invention has higher VOCs oxidation activity, for example, may have a lower VOCs conversion temperature.
[0018] The method for preparing a VOCs catalytic oxidation catalyst provided by the present invention reduces the hydrolysis rate of the noble metal by precisely controlling the pH of the noble metal cation hydrolysis process, and cooperates with appropriate preparation steps and conditions to increase the dispersion of the noble metal on the carrier surface, thereby obtaining a catalyst with high VOCs oxidation activity. The catalyst preparation method provided by the present invention has controllable and relatively uniform noble metal particle size, and the noble metal particle size can be adjusted by adjusting the pH value. The preparation method provided by the present invention is simple to operate and suitable for mass production.
[0019] The VOCs catalytic oxidation catalyst provided by the present invention is used to oxidize VOCs to generate CO2. At the same conversion rate, it can have a lower conversion temperature or a higher conversion rate at the same temperature. For example, the oxidation catalyst provided in Example 1 of the present invention is used for toluene oxidation, T 50 201℃, T 99 is 220.8℃.50 The lowest is 225.7℃, T 99 The minimum is 250.8℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a high-magnification transmission electron microscope image of the slurry after drying and calcination in Example 1
[0021] Figure 2 This is a high-magnification transmission electron microscope image of the slurry after drying and calcination in Comparative Example 1
[0022] contrast Figure 1 , Figure 2 It can be seen that the method of the present invention can significantly reduce the particle size of the precious metal and improve the dispersion of the precious metal. DETAILED DESCRIPTION
[0023] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0024] In the present invention, the noble metal is at least one selected from the group consisting of Pt, Pd, Ag and Rh.
[0025] The buffer reagent is preferably an organic acid that can make the mixed solution form a buffer solution with a pH value of 1.5-3.5, preferably 1.5-3.
[0026] In one embodiment, the buffering agent is an organic acid soluble in water with a pKa of 1.5 to 5.0, for example, 1.5 to 4.5, wherein the pKa is the pKa (ionization equilibrium constant of the organic acid) value at 25° C. and 1 atm. Preferably, the buffering agent is an organic acid free of sulfur and / or chlorine substituents. The buffering agent is preferably one or more of malonic acid, tartaric acid, glycolic acid, and butyric acid.
[0027] The alkali metal and / or alkaline earth metal as alkaline electron auxiliary agent can be selected from at least one of K, Na, Mg and Ca.
[0028] The VOCs catalytic oxidation catalyst contains a matrix, which can be at least one of alumina, aluminum-based spinel (for example, AB2O4 configuration, wherein B is aluminum or aluminum and other transition metals such as one or more of Cr and Fe, and A is a balancing metal such as an alkaline earth metal, one or more of Group IIB metals such as Mg and\or Zn), perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably at least one of alumina, spinel and perovskite, and more preferably alumina.
[0029] The matrix source is a substance that can be converted into a matrix under the calcination conditions of step (3). The matrix source is preferably a substance having surface hydroxyl groups, which can generate an oxide having a certain specific surface area and good thermal stability after calcination. For example, the matrix source is one or more of hydrated alumina, activated alumina, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite; the hydrated alumina is one or more of gibbsite, diaspore, gibbsite, boehmite and pseudo-boehmite; the activated alumina is one or more of ρ-alumina, χ-alumina, η-alumina, γ-alumina, κ-alumina, δ-alumina and θ-alumina.
[0030] Preferably, in the mixed solution of step (1), the mass concentration of the buffer reagent is 0.5%-5%, for example, 1.5%-3%.
[0031] Preferably, in the first mixed solution of step (1), the mass concentration of the noble metal precursor salt is 0.02%-0.6%, preferably 0.05%-0.4%.
[0032] Preferably, in the first mixed solution of step (1), the mass concentration of alkali metal and / or alkaline earth metal salt (alkali metal and / or alkaline earth metal are also collectively referred to as alkaline electron auxiliary agent) is 0.1%-0.9%, preferably 0.3%-0.6%.
[0033] In one embodiment, in the first mixed solution, the mass concentration of the matrix source on a dry basis is 5%-50%, preferably 10%-30%.
[0034] Preferably, in the first mixed solution of step (1), the ratio of the matrix source to water is 0.05:1-0.5:1, preferably 0.1:1-0.3:1 by mass.
[0035] According to the present invention, the noble metal ions are slowly hydrolyzed to perform a hydrolysis reaction. In one embodiment, the temperature for slowly hydrolyzing the noble metal ions is preferably 5 to 45°C.
[0036] In one embodiment of the present invention, the hydrolysis reaction is carried out for 0.5-3 hours at a pH value of 1.5-3.5, preferably 1.5-3. The buffer reagent is preferably an organic acid that can form a buffer solution with a pH value of 1.5-3.5.
[0037] In the present invention, the hydrolysis is carried out under the action of ultrasonic waves (also called ultrasonic stirring).
[0038] In the present invention, in step (1), the drying can be carried out according to conventional methods, preferably, the drying temperature does not exceed 140°C, such as 60-140°C. In one embodiment, evaporation is first performed, and then a second drying is performed; the conditions for evaporation include, for example, an evaporation temperature of 60-100°C, and evaporation is performed until the sample becomes viscous or the stirring rotor cannot rotate. The conditions for the second drying include: a drying temperature of 80-140°C, and in one embodiment, the second drying time is 4-12h.
[0039] According to the present invention, the ozone roasting conditions include: the roasting temperature is 150-300°C, the time is 1-3h; the roasting atmosphere contains ozone, and preferably, the ozone concentration in the roasting atmosphere is 0.5-1000ppm (volume).
[0040] In the present invention, the oxygen storage material is at least one of bismuth oxide, cerium oxide, cerium-zirconium solid solution, and niobium oxide, preferably bismuth oxide.
[0041] In the present invention, the binder can be selected from at least one of silica sol, alumina sol, acidic alumina such as pseudo-boehmite, preferably one or more of alumina sol and pseudo-boehmite. The binder becomes a matrix material after calcination, which is called a binder matrix.
[0042] Preferably, the catalyst slurry contains: the mass fraction of the matrix material loaded with active components on a dry basis is 4%-35%, preferably 8%-20%; the mass fraction of the oxygen storage material is 0.5%-4%, preferably 1%-3%; the mass fraction of zirconium acetate is 0.3%-2%, preferably 0.5%-1.5%; the mass fraction of the binder on a dry basis is 1%-5%, preferably 1.8%-3.5%.
[0043] In one embodiment, the solid content of the catalyst slurry is 5.8%-47.5% by mass.
[0044] In the present invention, in step (2), the average diameter of the particles in the catalyst slurry is less than 15 μm. The average diameter of the particles is measured by a laser particle size method in accordance with the NB / SH / T 0951-2017 industry standard.
[0045] In the present invention, the catalyst slurry loading amount is such that the loading amount of the catalyst layer is 20-140 g / L, preferably 30-100 g / L, based on the volume of the carrier. The loaded catalyst slurry is dried and calcined to form a catalyst layer.
[0046] In the present invention, the amount of each component is such that, based on the volume of the carrier, the loading amount of the precious metal is 0.05-2 g / L in terms of element, preferably 0.3-1.2 g / L; the loading amount of the matrix is 18-130 g / L in terms of oxide, preferably 35-85 g / L; the loading amount of the alkali metal or alkaline earth metal oxide is 0.2-2 g / L, preferably 0.6-1.2 g / L; the loading amount of the oxygen storage material oxide is 2-16 g / L, preferably 4-12 g / L; the loading amount of zirconium oxide is 0.7-5 g / L, preferably 1.5-3 g / L.
[0047] The present invention has a wide range of choices for the carrier, and can be various carriers conventionally used in the art, and the present invention has no particular limitation thereto. For example, the carrier can be an inorganic oxide carrier.
[0048] Preferably, the carrier is at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloy carriers.
[0049] The carrier of the present invention can be used to provide a catalyst bed in a fixed bed reactor. The carrier can be a whole carrier block with a hollow channel structure formed inside, active components can be distributed on the inner wall and / or outer wall of the channel, and the channel space can be used as a flow space for fluid.
[0050] Preferably, the carrier is a regular structure carrier, that is, the appearance of the carrier is a regular structure, which is easy to assemble, and the pore structure of the carrier can also be regular.
[0051] For example, the carrier may be a regular carrier having honeycomb-shaped openings in the cross section (referred to as a honeycomb carrier).
[0052] The openings of the regular carrier may be of regular or irregular shapes, and the shapes of the holes may be the same or different, and each hole may be independently in the shape of a square, an equilateral triangle, a regular hexagon, a circle, or a corrugated shape.
[0053] Preferably, the pore density of the cross section of the regular structure carrier is 50-400 pores / square inch, for example, it can be 50, 100, 150, 200, 250, 300, 350, 400 pores / square inch and any range between any two values.
[0054] Preferably, the cross-sectional area of each hole in the carrier is 0.4-10 square millimeters, preferably 0.4-4 square millimeters.
[0055] Preferably, the open porosity of the carrier surface is 20-80%, more preferably 50-80%.
[0056] In the present invention, the catalyst slurry can be evenly loaded on the surface of the carrier by spraying, coating or immersion, and then dried and calcined to obtain a carrier with catalyst layers loaded on the inner and outer surfaces. For example, the carrier can be immersed in the catalyst slurry for 5-30 seconds for loading.
[0057] It should be understood that in the present invention, the preferred conditions can be more conducive to improving the performance of the catalyst and enhancing the catalytic effect, such as lowering the VOCs oxidation temperature to achieve the same conversion rate or increasing the conversion rate at the same conversion temperature.
[0058] In the present invention, in step (3), the drying conditions include, for example, a temperature of 80-140° C. and a drying time of 0.5-4 h.
[0059] In step (3), the calcination treatment is preferably carried out under ozone conditions, which is called ozone calcination. The conditions for ozone calcination include: calcination temperature of 150-300° C., time of 1-3 hours. The ozone concentration in the calcination atmosphere can be, for example, 0.5-1000 ppm (volume).
[0060] The preparation method of the VOCs catalytic oxidation catalyst of the present invention, in one embodiment, comprises:
[0061] (1) mixing a buffer agent, an alkali metal and / or alkaline earth metal salt, a matrix source and water, and then adding a noble metal nitrate to form a first mixed solution, wherein the pH value of the first mixed solution is preferably 1.5-3.5, preferably 1.5-3, such as 1.5-2, slowly hydrolyzing the noble metal ions under ultrasonic stirring conditions, wherein the pH value after the hydrolysis is not more than 3.5, preferably not more than 3, drying, and ozone roasting to obtain an active component-loaded matrix material; the mass concentration of the buffer agent in the first mixed solution is 0.5%-5%;
[0062] (2) mixing the matrix material loaded with active components, the oxygen storage material, zirconium acetate and the binder with water, and ball milling to obtain a catalyst slurry;
[0063] (3) The catalyst slurry is loaded onto a carrier, and after drying and calcination, a VOCs catalytic oxidation catalyst loaded with a catalyst layer is obtained after ball milling.
[0064] The present invention will be described in detail below by way of examples. The following examples will further illustrate the present invention, but are not intended to limit the present invention.
[0065] The average diameter of the particles in the catalyst slurry is the equivalent volume diameter obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.
[0066] The activity evaluation of the catalytic oxidation reaction of toluene was completed on a micro-fixed bed reactor designed and manufactured by Tianjin Pengxiang Technology Co., Ltd., equipped with a Multigas 2030 infrared detector from MKS. The reaction was carried out at normal pressure, with an initial temperature of 150°C and a temperature program of 3°C / min until the VOCs pollutants were completely converted. The volume composition of the inlet gas was 450ppm C7H8 / 7% O2 / N2, and the volume space velocity was 12000h -1 .
[0067] The carrier is a VOC-specific cordierite honeycomb carrier purchased from Pingxiang Guanlin Environmental Protection Technology Co., Ltd. The carrier pore density is 300 holes / square inch, the cross-sectional area of each hole is 1.5 square millimeters, the open porosity is 70%, and the hole shape is circular.
[0068] The average particle size of the precious metal is measured by projection electron microscopy using a JEM2100F instrument. The maximum size value of the projection is the particle size of the particle. 30 particles are randomly selected and their average value is taken.
[0069] Example 1
[0070] (1) 10 g of malonic acid, 5 g of sodium nitrate, 250 g of γ-alumina (Zhengzhou Nonferrous Research Institute Co., Ltd., China Aluminum Corporation) and 750 g of water were mixed, and then 0.1 mol / L platinum nitrate aqueous solution (containing 2.5 g of platinum nitrate) was added. The initial pH of the mixed solution was 1.8. The precious metal was slowly hydrolyzed for 1.5 h under ultrasonic stirring (40000 Hz, 100 W) at 25 ° C. After the hydrolysis reaction, the pH increased slightly to 2.2. The mixture was evaporated to dryness in a water bath at 85 ° C. under stirring, and then dried at 120 ° C. for 6 h. The mixture was heated to 200 ° C. at a rate of 5 ° C. / min in an ozone atmosphere with an ozone concentration of 10 ppm (volume) and maintained for 2 h to obtain an active component-loaded matrix material;
[0071] (2) 240 g of the matrix material loaded with the active component, 40 g of bismuth oxide, 20 g of zirconium acetate, 50 g of diaspore (nitric acid-acidified pseudo-boehmite, the molar ratio of nitric acid to pseudo-boehmite calculated as Al2O3 is 0.04:1, solid content 20 wt%) and 2 L of water were mixed and stirred for 2 h. The mixture was fully ground using a vibrating ball mill (Tianjin Shengyuan Equipment Co., Ltd., GZM-6). The specific grinding conditions were: ball milling time 2.5 h, rotation speed 95 0rpm, the average particle diameter of the mixed liquid after ball milling is 9.8μm; then the catalyst slurry is evenly coated on the surface of a 300-mesh regular structure carrier, so that the total coating amount on each liter of ceramic carrier is 70g, and the precious metal loading is 0.4g / L in terms of elements, and the loading of aluminum oxide is 57.9g / L in terms of oxides, the loading of sodium oxide is 0.7g / L, the loading of bismuth oxide is 8.5g / L, and the loading of zirconium oxide is 2.5g / L.
[0072] (3) The carrier coated with the catalyst slurry was dried at 140°C for 2 hours, and then subjected to ozone calcination treatment, the temperature was raised to 180°C at a rate of 5°C / min, and maintained for 2 hours, the ozone concentration in the atmosphere was 10 ppm (volume), and a VOCs catalytic oxidation catalyst was obtained.
[0073] Example 2
[0074] In Example 2, in step (1), an equal mass of palladium nitrate is used to replace platinum nitrate, and an equal mass of tartaric acid is used to replace malonic acid. Other conditions are the same as in Example 1.
[0075] Example 3
[0076] In Example 3, an equal mass of butyric acid is used as a buffer reagent in step (1), and the pH of the slurry after hydrolysis is 3.5. Other conditions are the same as in Example 1.
[0077] Example 4
[0078] In Example 4, bismuth oxide is added in step (1), and other conditions are the same as those in Example 1.
[0079] Comparative Example 1
[0080] In Comparative Example 1, no buffer reagent was added in step (1), the pH of the slurry after hydrolysis was 4.8, and other conditions were the same as those in Example 1.
[0081] Comparative Example 2
[0082] Comparative Example 2: In step (1), an equal molar amount of sodium hexachloroplatinate was added to replace platinum nitrate, and other conditions were the same as those in Example 1.
[0083] Comparative Example 3
[0084] In Comparative Example 3, no sodium nitrate was added in step (1), and other conditions were the same as those in Example 1.
[0085] Comparative Example 4
[0086] In Comparative Example 4, bismuth oxide was not added in step (2), and other conditions were the same as those in Example 1.
[0087] Comparative Example 5
[0088] In comparative example 5, in step (3), the temperature is raised to 330°C at a rate of 5°C / min and maintained for 2 hours (since the oxidation performance of air is weaker than that of ozone, calcination at a temperature above 300°C is required to remove the organic matter in the precursor). Other conditions are the same as those in example 1.
[0089] The performance of the VOCs catalytic oxidation materials obtained in the examples and comparative examples was evaluated using toluene as a model compound. The results of the T50 and T99 conversion temperatures are shown in Table 1.
[0090] Table 1 T50, T99 and average particle size of precious metals for toluene oxidation of each catalyst sample, preparation and hydrolysis conditions
[0091]
[0092] As can be seen from Table 1, the T 50 and T 99 The toluene conversion temperature is lower than that of the comparative example, and the VOCs catalytic material prepared by the present invention has higher pollutant degradation efficiency.
[0093] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a VOCs catalytic oxidation catalyst, comprising the following steps: (1) mixing a buffer agent, an alkali metal and / or alkaline earth metal salt, an optional oxygen storage material, a matrix source and water, then adding a noble metal nitrate to form a first mixed solution, slowly hydrolyzing the noble metal ions under ultrasonic stirring and a pH value of 1.5-3.5, for example, 1.5-3, drying and ozone roasting to obtain a matrix material loaded with active components; the mass concentration of the buffer agent in the first mixed solution is 0.5%-5%, (2) mixing the matrix material loaded with active components, the optional oxygen storage material, zirconium acetate, the binder oxide and water, and grinding them to obtain a catalyst slurry; wherein the oxygen storage material is added in at least one of steps (1) and (2); (3) The catalyst slurry is loaded onto a carrier, dried and calcined to obtain a VOCs catalytic oxidation catalyst loaded with a catalyst layer.
2. The method according to claim 1, wherein: The noble metal is one or more of Pt, Pd, Ag and Rh; The buffer reagent is an organic acid soluble in water and having a pKa of 1.5 to 5.0, and the buffer reagent is preferably one or more of malonic acid, tartaric acid, glycolic acid, and butyric acid; The alkali metal and / or alkaline earth metal is one or more of K, Na, Mg and Ca.
3. The method according to claim 1, wherein: The matrix source is one or more of hydrated alumina, activated alumina, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite; the hydrated alumina is, for example, one or more of gibbsite, diaspore, nordstromite, diaspore, boehmite and pseudo-boehmite; the activated alumina is, for example, one or more of ρ-alumina, χ-alumina, η-alumina, γ-alumina, κ-alumina, δ-alumina and θ-alumina.
4. The method according to claim 1, wherein: Step (1) In the first mixed solution, the mass concentration of the noble metal precursor salt is 0.02%-0.6%, preferably 0.05%-0.4%; the mass concentration of the alkali metal and / or alkaline earth metal salt is 0.1%-0.9%, preferably 0.3%-0.6%; the mass concentration of the matrix source is 5%-50%, preferably 10%-30% on a dry basis; In the first mixed solution, the mass concentration of the buffer reagent is 1.5%-3%.
5. The method according to claim 1, wherein: In step (1), the precious metal ions are slowly hydrolyzed: the hydrolysis reaction is carried out at a pH value of 1.5-3.5 and ultrasonic action for 0.5-3h; the hydrolysis reaction temperature is preferably 5-45°C; the buffer reagent is preferably an organic acid that can form a buffer solution with a pH value of 1.5-3.
5.
6. The method according to claim 1, wherein: In step (1), the drying temperature is preferably not more than 140°C, and / or, In step (1), the conditions of ozone roasting include: roasting temperature of 150-300°C, time of 1-3h, ozone in the roasting atmosphere, and the ozone concentration in the roasting atmosphere is preferably 0.5-1000ppm by volume; and / or In step (3), the drying conditions include: a temperature of 80-140° C. and a time of 0.5-4 h; and / or In step (3), the calcination conditions include: a calcination temperature of 150-300° C. and a calcination time of 1-3 h; the calcination is preferably carried out in the presence of ozone, and the ozone concentration in the calcination atmosphere is preferably 0.5-1000 ppm by volume.
7. The method according to claim 1, wherein: The oxygen storage material is one or more of bismuth oxide, cerium oxide, cerium-zirconium solid solution, and niobium oxide; The binder is selected from one or more of silica sol, alumina sol and pseudo-boehmite; Preferably, in the catalyst slurry, the mass fraction of the matrix material loaded with active components is 4%-35%, preferably 8%-20%; the mass fraction of the oxygen storage material is 0.5%-4%, preferably 1%-3%; the mass fraction of zirconium acetate is 0.3%-2%, preferably 0.5%-1.5%; the mass fraction of the binder is 1%-5%, preferably 1.8%-3.5%; in one embodiment, the solid content of the catalyst slurry is 5.8%-47.5% by weight.
8. The method according to claim 1, wherein: In step (2), the average diameter of the particles in the catalyst slurry is less than 15 μm; the average diameter of the particles is measured by a laser particle size method in accordance with the NB / SH / T 0951-2017 industry standard.
9. The method according to claim 1, wherein: The carrier is a regular structure carrier, and the regular structure carrier is preferably a honeycomb carrier; preferably, the cross-section of the honeycomb carrier has a pore density of 50-400 pores / square inch and an open porosity of 20-80%.
10. The method according to claims 1 to 9, wherein: The catalyst slurry is loaded onto the carrier so that, based on the volume of the carrier, the loading amount of the catalyst layer in the VOCs catalytic oxidation catalyst loaded with the catalyst layer is 20-140 g / L, preferably 30-100 g / L.
11. The method according to any one of claims 1 to 10, wherein: The amount of each component is such that, based on the volume of the carrier, in the VOCs catalytic oxidation catalyst loaded with a catalyst layer, the loading amount of precious metals in terms of elements is 0.05-2g / L, selected as 0.3-1.2g / L; the loading amount of the matrix in terms of oxides is 18-130g / L, selected as 35-85g / L; the loading amount of alkali metal and / or alkaline earth metal oxides is 0.2-2g / L, selected as 0.6-1.2g / L; the loading amount of oxygen storage material oxides is 2-16g / L, selected as 4-12g / L; the loading amount of zirconium oxide is 0.7-5g / L, selected as 1.5-3g / L.
12. A VOCs catalytic oxidation catalyst prepared according to the method according to any one of claims 1 to 11.
13. A VOCs catalytic oxidation catalyst, comprising a carrier and a catalyst layer on the carrier, wherein: The catalyst layer comprises a matrix material loaded with active components, an oxygen storage material, zirconium oxide and a binder oxide, wherein the matrix material loaded with active components comprises a noble metal, an alkaline earth metal and / or an alkali metal, and a matrix; the average particle size of the noble metal in the matrix material loaded with active components is 1.4-2.4 nm; Preferably, the loading amount of precious metal is 0.05-2g / L, preferably 0.3-1.2g / L; in terms of oxide, the loading amount of the matrix is 18-130g / L, preferably 35-85g / L; the loading amount of alkali metal and / or alkaline earth metal oxide is 0.2-2g / L, preferably 0.6-1.2g / L; the loading amount of oxygen storage material oxide is 2-16g / L, preferably 4-12g / L; the loading amount of zirconium oxide is 0.7-5g / L, preferably 1.5-3g / L.
14. Use of the VOCs catalytic oxidation catalyst according to any one of claims 12 to 13 in the catalytic oxidation of VOCs.