Cobalt-cerium catalyst for catalyzing low-carbon alkane at low temperature as well as preparation method and application of cobalt-cerium catalyst

Through the preparation method of cobalt cerium catalyst, the existing transition metal catalysts have been solved, and the catalytic activity of low-temperature and efficient activation of low-carbon alkane degradation is achieved, and the efficiency and water resistance of low-temperature catalytic degradation of low-carbon alkanes are achieved. Good economics and industrial application potential.

CN119034752AActive Publication Date: 2024-11-29ZHEJIANG UNIV

Patent Information

Application Number
CN202411072984.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing transition metal catalysts have problems of insufficient stability and catalytic activity in the degradation of low-temperature and high-efficiency activation of low-carbon alkanes, which limits their use in industrial applications.

Method used

Using the preparation method of cobalt cerium catalyst, the cobalt salt and cerium salt precursor are dissolved in ultrapure water, controlled pH value, added and crystallized, and then roasted to obtain cobalt cerium catalyst, which has good low-temperature catalytic activity and cycle stability.

Benefits of technology

The high efficiency and water resistance of low-temperature catalytic degradation of low-carbon alkanes are achieved, and the cost of catalysts is reduced, and the cost of economics and industrial application potential is good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034752A_ABST
    Figure CN119034752A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a cobalt-cerium catalyst for catalyzing low-carbon alkane at low temperature, which comprises the following steps: dissolving a cobalt salt precursor and a cerium salt precursor in ultrapure water to obtain a solution A; naOH and Na2CO3 are dissolved in ultrapure water, and a solution B is obtained; under violent stirring at 40 DEG C, dropwise adding the solution A and the solution B into ultrapure water at the same time according to a proper dropwise adding speed; after the titration is finished, stirring the mixture and crystallizing for 10-15 hours; cooling the product to room temperature; filtering, washing and drying the obtained precipitate; and roasting the powder in a muffle furnace in an air atmosphere for 4-6 hours to obtain the cobalt-cerium catalyst. Compared with other transition metal catalysts, the cobalt-cerium catalyst has the remarkable low-temperature activity advantage, the operation cost of the catalyst in the using process can be reduced, meanwhile, the cobalt-cerium catalyst further has good cycling stability and water resistance, and good industrial application potential and prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a cobalt-cerium catalyst for catalyzing low-carbon alkanes at a low temperature, and a preparation method and application thereof. Background Art

[0002] Low-carbon alkanes refer to saturated alkanes with carbon atoms less than or equal to 4, namely methane, ethane, propane and butane, which are typical greenhouse gases. Low-carbon alkanes emitted into the atmosphere will react with nitrogen oxides in the air to produce photochemical smog and ozone, causing problems such as global climate deterioration and directly endangering human health. Therefore, it is urgent to effectively remove low-carbon chain alkanes directly emitted into the atmosphere to avoid the environmental problems they bring.

[0003] Due to the high bond energy of the CH bond of low-carbon alkanes and their stable chemical properties, their low-temperature and efficient activation and catalytic degradation is a hot topic and challenge in current research. Precious metal catalysts have good oxidation properties, but they are limited by cost and service life, and there is an urgent need to develop high-quality catalysts that can be replaced with good economy. Among them, transition metal oxides have good catalytic activity for the catalytic combustion of VOCs comparable to that of precious metal catalysts, and are economical, and are the mainstream direction of future catalyst research and development. However, most of the existing transition catalysts still have the disadvantages of stability and insufficient catalytic activity, which limits their actual industrial production. In view of this, it is of great significance to develop a transition metal cobalt-cerium catalyst for the degradation of low-carbon alkanes to solve the problems existing in existing transition metal catalysts. Summary of the invention

[0004] In order to solve one of the above problems, the present invention provides a cobalt-cerium catalyst for low-carbon alkane catalysis at low temperature, and a preparation method and application thereof. The cobalt-cerium catalyst has good low-temperature conversion activity and cycle stability for the catalytic degradation of short-chain alkanes, and has good water resistance, good economic value and industrial application value.

[0005] In order to achieve the above object, the present invention adopts the following technical means: The first aspect of the present invention provides a method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature, comprising the following steps: (1) dissolving a cobalt salt precursor and a cerium salt precursor in ultrapure water to obtain a solution A; (2) Dissolve NaOH and Na2CO3 in ultrapure water to obtain solution B; (3) under vigorous stirring at 40° C., solution A obtained in (1) and solution B obtained in (2) are simultaneously added dropwise into ultrapure water at an appropriate dropping speed; (4) After the titration is completed, the mixture formed in (3) is stirred and crystallized for 10-15 h; (5) After the product in (4) is cooled to room temperature, the precipitate obtained is filtered, washed and dried; (6) The powder obtained in (5) is calcined in a muffle furnace under air atmosphere for 4-6 h to obtain a cobalt-cerium catalyst.

[0006] In an embodiment of the present invention, in the cobalt salt precursor and the cerium salt precursor in step (1), the molar ratio of Co / Ce is (0.3-5): 1. In some preferred embodiments of the present invention, the molar ratio of Co / Ce is (3-5): 1; more preferably, the molar ratio of Co / Ce is 3:1.

[0007] In an embodiment of the present invention, the amount of Na2CO3 in step (2) is twice that of the cerium salt precursor; the amount of NaOH is twice that of the cobalt salt precursor and the cerium salt precursor, and the volumes of solution A and solution B are the same.

[0008] In an embodiment of the present invention, the appropriate dropping speed in step (3) is to maintain the pH value of the solution after dropping at 10±0.2.

[0009] In an embodiment of the present invention, the stirring time in step (4) is 30-60 min, and the crystallization temperature is 60-80°C.

[0010] In the embodiment of the present invention, the washing method in step (5) is: washing by centrifugation with deionized water until the filtrate is neutral, and the drying temperature is 60-80°C.

[0011] In an embodiment of the present invention, in step (6), the air flow rate is 50-100 mL / min, and the calcination temperature is 300-450°C.

[0012] The second aspect of the present invention provides a cobalt-cerium catalyst prepared by the method described in the first aspect.

[0013] The third aspect of the present invention provides the use of the cobalt-cerium catalyst described in the second aspect in the degradation of low-carbon alkane pollutants in the atmosphere.

[0014] In some embodiments of the present invention, the low carbon alkanes include propane, ethane, and methane.

[0015] In some embodiments of the present invention, the present invention further provides the use of the cobalt-cerium catalyst described in the second aspect in the low-temperature catalytic degradation of propane. The catalytic degradation temperature of propane is lower than 200 °C, and the mass space velocity during the catalytic degradation is 30000-120000 mL·g -1 ·h -1 The application also includes the application of catalytic degradation of propane under wet conditions.

[0016] Beneficial Effects of the Invention Compared with the prior art, the present invention has the following beneficial effects: the present invention uses transition metal cobalt cerium as raw material, which greatly saves costs compared with precious metal catalysts and has good economic efficiency. The cobalt cerium metal catalyst prepared by the invention has significant low-temperature activity advantages compared with other transition metal catalysts, and can reduce the operating cost of the catalyst use process. At the same time, it also has good cycle stability and water resistance, has good industrial application potential and prospects, and can be widely used in the field of efficient degradation of low-carbon alkanes in the atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Shows the SEM images of the catalysts prepared in Examples 1-4; Figure 2 The XRD characterization diagrams of the catalysts prepared in Examples 1-4 are shown; Figure 3 The propane degradation performance comparison results of the catalysts prepared in Examples 1-4 under dry conditions are shown; Figure 4 The propane degradation performance comparison results of the catalysts prepared in Examples 1-4 under wet conditions are shown; Figure 5 The graph showing the change of propane conversion rate of the catalyst prepared in Example 3 at different weight hourly space velocities as a function of temperature is shown; Figure 6 The figure shows the cycle performance test result of the catalyst prepared in Example 3; Figure 7 A comparative diagram showing the catalytic degradation of methane, ethane and propane by the catalyst prepared in Example 3 is shown; Figure 8 A comparison diagram of propane degradation under dry conditions by the catalysts prepared in Example 3, Comparative Example 1 and Comparative Example 2 is shown; wherein Comparative Example 1 is a hydrothermal method, Comparative Example 2 is a single titration method, and Example 3 is a double titration method; Fig. 9 A comparison diagram of propane degradation under wet conditions by the catalysts prepared in Example 3, Comparative Example 1 and Comparative Example 2 is shown; wherein Comparative Example 1 is a hydrothermal method, Comparative Example 2 is a single titration method, and Example 3 is a double titration method; Fig.10 The figure shows a comparison of the long-term stable catalytic performance of the catalysts prepared in Example 2 and Example 3 under humid conditions. DETAILED DESCRIPTION

[0018] The following examples are used to demonstrate preferred embodiments of the present invention. It will be appreciated by those skilled in the art that the techniques disclosed in the following examples represent techniques discovered by the inventors that can be used to implement the present invention and therefore can be considered as preferred embodiments of the present invention. However, it will be appreciated by those skilled in the art based on this specification that many modifications may be made to the specific embodiments disclosed herein and still achieve the same or similar results without departing from the spirit or scope of the present invention.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs, and the materials cited herein and those cited by them are incorporated by reference. Those skilled in the art will recognize or will learn through routine experimentation that there are many equivalents to the specific embodiments of the invention described herein. Such equivalents are intended to be encompassed by the claims.

[0020] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.

[0021] A method for preparing a cobalt-cerium catalyst comprises the following steps: (1) dissolving a cobalt salt precursor and a cerium salt precursor in ultrapure water to obtain a solution A; wherein the molar ratio of Co / Ce in the cobalt salt precursor and the cerium salt precursor is (0.3-5):1; (2) Dissolve NaOH and Na2CO3 in ultrapure water to obtain solution B; wherein the amount of Na2CO3 is twice that of the cerium salt precursor; the amount of NaOH is twice that of the cobalt salt precursor and the cerium salt precursor, and the volumes of solution A and solution B are the same; (3) Under vigorous stirring at 40°C, solution A obtained in (1) and solution B obtained in (2) are simultaneously added dropwise into ultrapure water at an appropriate dropping rate to maintain the pH value of the solution at 10±0.2; (4) After the titration is completed, the mixture formed in (3) is stirred and crystallized for 10-15 h; the stirring time is 30-60 min, and the crystallization temperature is 60-80 °C; (5) After the product in (4) is cooled to room temperature, the precipitate obtained is filtered, washed by centrifugation with deionized water until the filtrate is neutral, and dried at 60-80 °C; (6) The powder obtained in (5) is calcined in a muffle furnace at an air flow rate of 50-100 mL / min and a temperature of 300-450°C for 4-6 h to obtain a cobalt-cerium catalyst.

[0022] Example 1 0.003 mol of cobalt nitrate hexahydrate and 0.009 mol of cerium nitrate hexahydrate were dissolved in 25 mL of ultrapure water to obtain solution A. 0.024 mol of NaOH and 0.018 mol of Na2CO3 were dissolved in 25 mL of ultrapure water to obtain solution B. Under vigorous stirring at 40 °C, solution A and solution B were simultaneously added dropwise to 25 mL of ultrapure water, and the pH of the solution was ensured to be 10 by controlling the dropping speed. After the titration, the mixture was stirred for 35 min, then the stirring was stopped and crystallized at 70 °C for 12 h. After cooling to room temperature, the obtained precipitate was filtered, washed to pH=7, dried at 70 °C for 12 h, and the obtained powder was calcined in a muffle furnace at 300 °C in an air atmosphere for 5 h to prepare a cobalt-cerium catalyst: Co1Ce3 catalyst.

[0023] Example 2 0.006 mol of cobalt nitrate hexahydrate and 0.006 mol of cerium nitrate hexahydrate were dissolved in 25 mL of ultrapure water to obtain solution A. 0.024 mol of NaOH and 0.012 mol of Na2CO3 were dissolved in 25 mL of ultrapure water to obtain solution B. Under vigorous stirring at 40 °C, solution A and solution B were simultaneously added dropwise to 25 mL of ultrapure water, and the pH of the solution was ensured to be 10 by controlling the dropping speed. After the titration, the mixture was stirred for 35 min, then the stirring was stopped and crystallized at 70 °C for 12 h. After cooling to room temperature, the obtained precipitate was filtered, washed to pH=7, and dried at 70 °C for 12 h. The powder was calcined in a muffle furnace at 300 °C in an air atmosphere for 5 h to prepare a cobalt-cerium catalyst: Co1Ce1 catalyst.

[0024] Example 3 0.009 mol of cobalt nitrate hexahydrate and 0.003 mol of cerium nitrate hexahydrate were dissolved in 25 mL of ultrapure water to obtain solution A. 0.024 mol of NaOH and 0.006 mol of Na2CO3 were dissolved in 25 mL of ultrapure water to obtain solution B. Under vigorous stirring at 40 °C, solution A and solution B were simultaneously added dropwise to 25 mL of ultrapure water, and the pH of the solution was ensured to be 10±0.2 by controlling the dropping speed. After the titration, the mixture was stirred for 35 min, then the stirring was stopped and crystallized at 70 °C for 12 h. After cooling to room temperature, the obtained precipitate was filtered, washed to pH=7, and dried at 70 °C for 12 h. The powder was calcined in a muffle furnace at 300 °C in an air atmosphere for 5 h to prepare a cobalt-cerium catalyst: Co3Ce1 catalyst.

[0025] Example 4 0.010 mol of cobalt nitrate hexahydrate and 0.002 mol of cerium nitrate hexahydrate were dissolved in 25 mL of ultrapure water to obtain solution A. 0.024 mol of NaOH and 0.004 mol of Na2CO3 were dissolved in 25 mL of ultrapure water to obtain solution B. Under vigorous stirring at 40 °C, solution A and solution B were simultaneously added dropwise to 25 mL of ultrapure water, and the pH of the solution was ensured to be 10 by controlling the dropping speed. After the titration, the mixture was stirred for 35 min, then the stirring was stopped and crystallized at 70 °C for 12 h. After cooling to room temperature, the obtained precipitate was filtered, washed to pH=7, and dried at 70 °C for 12 h. The powder was calcined in a muffle furnace at 300 °C in an air atmosphere for 5 h to prepare a cobalt-cerium catalyst: Co5Ce1 catalyst.

[0026] Comparative Example 1 The Co3Ce1 catalyst was prepared by a hydrothermal method as follows: Take 0.03 mol Co(NO3)3·6H2O and 0.01 mol Ce(NO3)3·6H2O and dissolve them in 100 mL ultrapure water; 0.1 mol CO(NH2)2 is dissolved in 100 mL ultrapure water. The two solutions are mixed together and transferred to a reactor, reacted at 110℃ for 24 h, washed with ultrapure water and anhydrous ethanol, and the resultant is vacuum dried at 60℃ for 12 h. The obtained powder is calcined at 300℃ in air for 5 h to finally prepare Co3Ce1 hydrothermal catalyst.

[0027] Comparative Example 2 The Co3Ce1 catalyst was prepared by single titration method as follows: Take 25 mL of 0.3 mol / L Co(NO3)3·6H2O and 0.1 mol / L Ce(NO3)3·6H2O salt solutions and place them in a 250 mL flask. Take a certain amount of NaOH and Na2CO3 to prepare 100 mL of alkali solution. Add the alkali solution to the salt solution at a certain speed while vigorously stirring the mixed salt solution. Add dropwise for about 45 minutes. After the pH of the solution reaches 10±0.1, stir for 10 minutes until the pH of the solution remains constant. Crystallize in a 90 ℃ water bath for 6 h to form a flocculent blue suspension. After cooling, filter out the supernatant, wash the precipitate with deionized water, centrifuge 4~5 times (until the pH is 7.0±0.5), dry the precipitate at 60 ℃ for 12 h, and calcine the obtained powder at 300 °C in air for 5 h to finally prepare the Co3Ce1 single titration catalyst.

[0028] Performance Testing and Characterization (1) The physical and chemical properties of the catalysts prepared in Examples 1-4 were tested under the same conditions. The results are shown in Table 1.

[0029] Table 1 Physical and chemical properties of the catalysts prepared in Examples 1-4

[0030] The results in the above table show that Co3Ce1 has the highest specific surface area and better low-temperature catalytic activity compared with other catalysts.

[0031] (2) The catalysts prepared in Examples 1-4 were subjected to SEM and XRD characterization tests. The results are as follows: Figure 1 and Figure 2 shown.

[0032] Depend on Figure 1 It can be seen that with the increase of Co / Ce ratio, the shape of the catalyst changes from strip to block, and Co3Ce1 presents uniform hexagonal flakes with high aspect ratio; the obtained lattice spacings of CeO2 (111), Co3O4 (220) and Co3O4 (311) are 0.31 nm, 0.29 nm and 0.24 nm respectively.

[0033] (3) The catalysts prepared in Examples 1-4 were tested for propane degradation performance under dry conditions and wet conditions. The results are as follows: Figure 3 and Figure 4 shown.

[0034] The results show that Figure 3 It can be seen that Co3Ce1 and Co5Ce1 have the best catalytic conversion efficiency for propane. Figure 4 It can be seen that under humid conditions, the catalytic performance of Co1Ce3 and Co1Ce1 for propane decreases significantly, while the catalytic performance of Co3Ce1 and Co5Ce1 for propane is more stable.

[0035] (4) The propane conversion rate of the catalyst prepared in Example 3 at different weight hourly space velocities is shown in the figure below: Figure 5 shown.

[0036] The results showed that at 30000 mL·g -1 ·h -1 、60000 mL·g -1 ·h -1 、120000 mL·g -1 ·h -1 The T90 temperatures of the catalysts at three different weight space velocities were 193 °C, 210 °C, and 221 °C, respectively. -1 ·h -1 Under these conditions, Co3Ce1 catalyzed propane conversion has a lower catalytic temperature.

[0037] (5) The catalyst prepared in Example 3 was subjected to a recycling experiment. The results are as follows: Figure 6 shown.

[0038] The results show that after the Co3Ce1 catalyst is recycled five times, the catalytic performance changes little, showing excellent cycle performance.

[0039] (6) The catalyst prepared in Example 3 was used to carry out catalytic experiments on methane, ethane and propane. The catalytic conversion results are as follows: Figure 7 shown.

[0040] The results show that the Co3Ce1 catalyst has a lower catalytic conversion temperature for propane, and the T90 temperature is below 200 ℃.

[0041] (7) The catalysts prepared in Example 3, Comparative Example 1 and Comparative Example 2 were subjected to propane degradation experiments under dry conditions and wet conditions. The performance curves of different catalysts for propane degradation are shown in FIG. Figure 8 and Fig. 9 shown.

[0042] The results show that the propane conversion rates of the catalysts prepared by the double titration method in Example 3, the hydrothermal method in Comparative Example 1, and the single titration method in Comparative Example 2 are not much different under dry conditions and at different temperatures. Figure 8 As shown in the figure, the T90 temperature is below 200°C. However, under humid conditions, the catalyst prepared by the double titration method of Example 3 has stable performance, and the T90 temperature is still below 200°C. However, the catalyst prepared by the hydrothermal method of Comparative Example 1 and the single titration method of Comparative Example 2 has poor performance stability, and the T90 temperature rises to above 200°C. This shows that the Co3Ce1 catalyst prepared by the double titration method has better water resistance.

[0043] (8) The catalysts prepared in Examples 2 and 3 were precipitated at a propane concentration of 2000 ppm and a mass space velocity of 30000 mL·g -1 ·h -1 , under the condition of reaction temperature of 225 ℃, 5 vol% H2O was added to test the catalyst stability. The results are as follows Fig.10 shown.

[0044] The results show that compared with Co1Ce1, the catalytic performance of Co3Ce1 under humid conditions remains almost unchanged, showing excellent stability and better water resistance.

[0045] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as references separately. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined in the present application.

Claims

1. A method for preparing a cobalt-cerium catalyst for low-carbon alkane catalysis at low temperature, characterized in that: The steps include: (1) dissolving a cobalt salt precursor and a cerium salt precursor in ultrapure water to obtain a solution A; (2) Dissolve NaOH and Na2CO3 in ultrapure water to obtain solution B; (3) Under vigorous stirring at 40°C, solution A obtained in (1) and solution B obtained in (2) are simultaneously added dropwise into ultrapure water at an appropriate dropping speed; (4) After the titration is completed, the mixture formed in (3) is stirred and crystallized for 10-15 h; (5) After the product in (4) is cooled to room temperature, the precipitate obtained is filtered, washed and dried; (6) The powder obtained in (5) is calcined in a muffle furnace under air atmosphere for 4-6 h to obtain a cobalt-cerium catalyst.

2. The method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: In step (1), the molar ratio of Co / Ce in the cobalt salt precursor and the cerium salt precursor is (0.3-5):

1.

3. The method for preparing the cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: In step (2), the amount of Na2CO3 is twice that of the cerium salt precursor; the amount of NaOH is twice that of the cobalt salt precursor and the cerium salt precursor, and the volumes of solution A and solution B are the same.

4. The method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: The appropriate dropping speed in step (3) is to maintain the pH value of the solution after dropping at 10±0.

2.

5. The method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: In step (4), the stirring time is 30-60 min and the crystallization temperature is 60-80 °C.

6. The method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: The cleaning method in step (5) is: centrifugal cleaning with deionized water until the filtrate is neutral, and the drying temperature is 60-80 °C.

7. The method for preparing a cobalt-cerium catalyst for catalyzing low-carbon alkanes at low temperature according to claim 1, characterized in that: In step (6), the air flow rate is 50-100 mL / min, and the calcination temperature is 300-450 °C.

8. The cobalt-cerium catalyst prepared by the method according to any one of claims 1 to 7.

9. Use of the cobalt-cerium catalyst according to claim 8 in the degradation of low-carbon alkane pollutants in the atmosphere.

10. The use according to claim 9, characterized in that: The low carbon alkanes include propane, ethane and methane.

Citation Information

Patent Citations

  • Preparation method of cobalt-cerium composite oxide catalyst and cobalt-cerium composite oxide catalyst

    CN105214675A

  • Monolithic catalyst for low temperature catalytic oxidation of carbon monoxide and preparation method thereof

    CN105289653A

  • Catalyst for cooperative control of multiple pollutants in waste incineration flue gas and preparation method and application of catalyst

    CN106378138A

  • Preparation, regeneration and application of catalyst for oxidation of volatile organic compounds

    CN106378211A

  • Preparation and regeneration method of VOCs low-temperature oxidation catalyst

    CN117884134A

Cited By

  • Cobalt-nickel catalyst for low-temperature catalytic degradation of VOCs and preparation method of cobalt-nickel catalyst

    CN119680547A

  • A cobalt-nickel catalyst for catalytic degradation of VOCs at low temperature and a preparation method thereof

    CN119680547B

  • Platinum-based catalyst for catalytic degradation of short-chain hydrocarbon VOCs and preparation method of platinum-based catalyst

    CN119897129A

  • Short-chain hydrocarbon VOCs catalytic degradation platinum-based catalyst and preparation method thereof

    CN119897129B