Supported nickel-based amorphous alloy catalyst as well as preparation method and application thereof

The supported nickel-based amorphous alloy catalyst Ni-Mo-P/SiO2 was prepared by impregnation-chemical reduction, which solved the problems of many by-products, high cost and complex preparation in the catalytic hydrogenation reaction of castor oil, and achieved high activity, The catalytic effect of long life and reaction at room temperature is suitable for industrial production.

CN119034770APending Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411061710.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, castor oil catalytic hydrogenation reaction has problems such as many by-products, high catalyst cost, complex catalyst preparation process, long experimental cycle, and high-temperature reduction equipment.

Method used

The supported nickel-based amorphous alloy catalyst Ni-Mo-P/SiO2 is prepared by impregnation-chemical reduction method. By adjusting the content of P, the electronic structure of Ni atoms is changed, the selectivity and activity of the catalyst are improved, and the Mo metal is introduced to make the catalyst. The dispersion is more uniform, simplifies the preparation process and reduces costs.

Benefits of technology

The prepared catalyst has high selectivity, high activity, few by-products, long service life, is suitable for industrial production, can react at room temperature, and can restore catalytic activity through simple activation and regeneration, and the product quality index meets national standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034770A_ABST
    Figure CN119034770A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a supported nickel-based amorphous alloy catalyst, which comprises the following steps: adding water to dissolve nickel salt, molybdate and sodium acetate to obtain a solution A; adding water to dissolve sodium hypophosphite monohydrate to obtain a solution B; pouring the solution A and the solution B into a container filled with silicon dioxide, stirring, and slowly dropwise adding sodium borohydride for reaction; and carrying out suction filtration on the turbid liquid obtained by the reaction, and carrying out stirring, suction filtration and drying on a filter cake to obtain the amorphous alloy catalyst. According to the Ni-Mo-P / SiO2 amorphous alloy catalyst prepared through the method, the electronic structure of Ni atoms can be changed by adjusting the content of P, then the high-selectivity and high-activity catalyst is prepared, Mo metal is introduced, the catalyst is dispersed more evenly, and the utilization rate of active components is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a supported nickel-based amorphous alloy catalyst and a preparation method and application thereof. Background Art

[0002] Castor bean is one of the top ten oil crops in the world and is a special industrial oil source crop. Castor oil is the only one that contains hydroxy acid (12-hydroxy-9-octadecenoic acid, molecular formula C 18 H 34 O3, commonly known as ricinoleic acid) is an industrial oil whose main component is ricinoleic acid. The hydroxyl groups in the ricinoleic acid molecular structure are easy to associate and form hydrogen bonds, so its viscosity is 8-10 times greater than that of general vegetable oil.

[0003] Hydrogenated castor oil is one of the important derivatives of castor oil. It is not only widely used in the cosmetics field, but also can be combined with lithium hydroxide to form lithium-based lubricants. It is widely used in aviation, automobiles, mechanical processing and other fields. In addition, hydrogenated castor oil is a raw material for many chemical reactions and is prone to cracking, esterification, amidation and hydrolysis. The hydrogenation reaction of castor oil occurs on the ninth double bond of ricinoleic acid. The reaction of castor oil requires catalytic hydrogenation of the olefin bond while keeping the hydroxyl unchanged. The reaction formula of castor oil catalytic hydrogenation is as follows: Figure 1 As shown. At present, there are two main castor oil catalytic hydrogenation process routes at home and abroad: 1) The use of traditional heterogeneous catalytic hydrogenation-heterogeneous catalytic addition reaction is a castor oil hydrogenation process widely used in industry; 2) Catalytic transfer hydrogenation (CTH) is a fat hydrogenation process using organic solution as a hydrogen donor. The hydrogenation catalysts used in traditional heterogeneous catalytic processes are mostly Ni-based metal catalysts prepared by coprecipitation. The preparation process of this type of catalyst is complicated, the experimental cycle is long, and high-temperature reduction equipment is required. In the catalytic transfer process, precious metals are often used as hydrogenation catalysts, but there are many by-products and the catalyst cost is high. In the CTH process, organic solutions are used as hydrogen donor solvents. These organic solutions need to be removed from the product through special chemical purification processes, which increases the complexity of the subsequent hydrogenation process. Therefore, the research on castor oil hydrogenation catalysts with simple preparation methods, high activity, and high selectivity and the development of simple hydrogenation processes are the current research focuses.

[0004] Amorphous alloys have more surface active centers, which are conducive to the adsorption of reactants and belong to the metastable state in thermodynamics. In recent years, catalyst technology has made important progress, especially in the field of metal catalysis. In the field of metal catalysis, nickel-based amorphous alloy catalysts are the main ones, which have fast reaction rates, high selectivity, and weaken the formation of trans fatty acids in oil hydrogenation. Therefore, they have great potential in oil catalytic applications. Summary of the invention

[0005] The purpose of the present invention is to provide a supported nickel-based amorphous alloy catalyst and a preparation method and application thereof, which are used to solve the technical problems in the prior art of castor oil catalytic hydrogenation reaction, such as the presence of a large number of by-products, high catalyst cost, complex catalyst preparation process, long experimental cycle, and the need for high-temperature reduction equipment.

[0006] To achieve the above object, one embodiment of the present invention provides a method for preparing a supported nickel-based amorphous alloy catalyst, comprising the following steps:

[0007] Add water to dissolve nickel salt, molybdate and sodium acetate to obtain solution A;

[0008] Add water to dissolve sodium hypophosphite monohydrate to obtain solution B;

[0009] Pour solution A and solution B into a container filled with silicon dioxide and stir, then slowly drop sodium borohydride to react;

[0010] The suspension obtained by the reaction is filtered, and the filter cake is stirred, filtered and dried to obtain an amorphous alloy catalyst.

[0011] In one of the preferred embodiments of the present invention, the amount of nickel salt added is 0.03 mol-0.05 mol, the amount of molybdate added is 0.05 mmol-0.40 mmol, and the amount of sodium acetate added is 0.01 mol-0.03 mol.

[0012] In one of the preferred embodiments of the present invention, the nickel salt is any one of nickel nitrate, nickel sulfate, nickel acetate and nickel chloride, and the molybdate includes ammonium heptamolybdate or sodium molybdate.

[0013] In one of the preferred embodiments of the present invention, the amount of sodium hypophosphite monohydrate added is 0.03 mol-0.05 mol.

[0014] One of the preferred embodiments of the present invention is to dropwise add sodium borohydride under a nitrogen atmosphere, wherein the amount of sodium borohydride added is 0.1 ml and the concentration is 2 mol / L.

[0015] In one preferred embodiment of the present invention, the filter cake obtained after the suspension is filtered is stirred with water and then filtered, and then stirred with ethanol and then filtered, and then dried to obtain the amorphous alloy catalyst.

[0016] Based on a supported nickel-based amorphous alloy catalyst disclosed in the present invention, the present invention also discloses a supported nickel-based amorphous alloy catalyst, which is prepared by the above-mentioned preparation method, and the supported nickel-based amorphous alloy catalyst is Ni-Mo-P / SiO2.

[0017] The invention also discloses an application of a supported nickel-based amorphous alloy catalyst. The supported nickel-based amorphous alloy catalyst is applied to catalytic hydrogenation of castor oil to synthesize hydrogenated castor oil.

[0018] One of the preferred schemes of the present invention is to synthesize hydrogenated castor oil by catalytic hydrogenation of castor oil, which comprises the following steps: adding castor oil and a catalyst into an autoclave, venting and replacing, adjusting the speed of the autoclave, heating and injecting hydrogen to react, removing hydrogen after the reaction is completed, cooling, and obtaining hydrogenated castor oil.

[0019] In one of the preferred solutions of the present invention, the venting pressure is 0.01 MPa, the speed of the reactor is 800 r / min-1200 r / min, the heating temperature is 140° C.-180° C., and the reaction time is 0.8 h-1.2 h.

[0020] In summary, the beneficial effects of the present invention are:

[0021] 1. The Ni-Mo-P / SiO2 amorphous alloy catalyst prepared by the present invention can change the electronic structure of Ni atoms by adjusting the P content, thereby preparing a highly selective and highly active catalyst, and the introduction of Mo metal makes the catalyst more evenly dispersed, thereby improving the utilization rate of the active components.

[0022] 2. The present invention adopts an impregnation-chemical reduction method to prepare a Ni-Mo-P / SiO2 amorphous alloy catalyst, which has a simple preparation process, cheap and readily available raw materials, high catalytic activity, few by-products, long service life, and easy regeneration. It is more suitable for industrial production and solves the problems that the preparation methods of existing castor oil catalytic hydrogenation catalysts are generally complicated, have a long preparation cycle, poor stability, are easy to oxidize and difficult to preserve.

[0023] 3. The various quality indicators of hydrogenated castor oil products prepared by the catalyst prepared by the present invention meet the national standards (iodine value ≤ 5.0g / 100g; hydroxyl value 150mg / g-165mg / g). In addition, after 50h of continuous production, the catalytic activity of the catalyst prepared by the present invention is 90% of that of the fresh catalyst; after 100h of continuous production, the catalytic activity is 85% of that of the fresh catalyst. The catalytic activity of the used catalyst can be restored to more than 97% of that of the fresh catalyst through simple activation and regeneration.

[0024] 4. Castor oil contains hydroxyl groups, and its hydrogenation products are greatly affected by the catalyst and reaction temperature, so high requirements are placed on the selectivity and activity of the catalyst. The use of traditional non-precious metal catalysts (such as Raney nickel, nickel-copper binary catalysts, etc.) requires high-temperature calcination and reduction of the catalyst, which places high requirements on equipment; the use of precious metal catalysts (such as palladium carbon, etc.) has high catalyst costs and produces more side reaction products. The Ni-Mo-P / SiO2 amorphous alloy catalyst prepared by the present invention breaks through the conditions for the hydrogenation catalytic reduction of castor oil, can react at room temperature, and does not need to undergo a high-temperature activation process subsequently. The preparation method is simple and does not require high-temperature calcination and reduction.

[0025] 5. The synthetic raw materials and reagents used in the present invention are relatively common and easily available, which is conducive to the large-scale production and application of the catalyst. The synthetic method uses less organic solvents and environmentally friendly conditions, reducing the impact on the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The reaction formula of catalytic hydrogenation of castor oil in one embodiment of the present invention is:

[0027] Figure 2 The present invention is a flow chart of a method for preparing a supported nickel-based amorphous alloy catalyst in one embodiment of the present invention;

[0028] Figure 3 The reaction flow chart of catalytic hydrogenation of castor oil in one embodiment of the present invention;

[0029] Figure 4 This is a diagram showing the properties of a supported nickel-based amorphous alloy catalyst in one embodiment of the present invention;

[0030] Figure 5 The present invention is an embodiment of the present invention, the catalyst prepared by Example 1 and Comparative Examples 1-3 is shown in scanning electron microscope micrographs, wherein (a) is a scanning electron microscope micrograph of carrier SiO2, (b) is a scanning electron microscope micrograph of Ni-P / SiO2, (c) is a scanning electron microscope micrograph of Ni-B / SiO2, (d) is a scanning electron microscope micrograph of Ni-BP / SiO2, and (e) is a scanning electron microscope micrograph of Ni-Mo-P / SiO2;

[0031] Figure 6 This is a diagram showing the properties of a hydrogenated castor oil product prepared under the action of a Ni-Mo-P / SiO2 catalyst in one embodiment of the present invention;

[0032] Figure 7 This is a gas chromatogram of a hydrogenated castor oil product prepared under the action of a Ni-Mo-P / SiO2 catalyst in one embodiment of the present invention.

[0033] Among them, 1-N2 bottle, 2-H2 bottle, 3-fixture, 4-thermocouple, 5-autoclave. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing a supported nickel-based amorphous alloy catalyst, such as Figure 2 As shown, the following steps are included:

[0035] Step (1): adding water to dissolve nickel salt, molybdate and sodium acetate to obtain solution A; specifically, weighing 0.03 mol-0.05 mol of nickel salt, 0.05 mmol-0.40 mmol of molybdate, and 0.01 mol-0.03 mol of CH3COONa (sodium acetate) into a 500 ml beaker, adding the mixture to 240 ml of distilled water and dissolving the mixture to obtain solution A;

[0036] Step (2): adding water to dissolve sodium hypophosphite monohydrate to obtain solution B; specifically, weighing 0.03 mol-0.05 mol of NaH2PO2·H2O (sodium hypophosphite monohydrate) into a 5 ml beaker, adding 7 ml of distilled water to dissolve, to obtain solution B;

[0037] Step (3): Pour solution A and solution B into a container containing silicon dioxide and stir, and slowly add sodium borohydride dropwise to react; specifically, weigh 10 g of SiO2 (silicon dioxide) into a 500 ml three-necked flask, pour solution A and solution B into the three-necked flask containing SiO2 and stir vigorously, and slowly add 0.1 ml of 2 mol / L NaBH4 solution (as an initiator) dropwise under a nitrogen atmosphere until no bubbles are generated in the solution, indicating that the reaction is complete.

[0038] Step (4): Filter the suspension obtained by the reaction, and obtain an amorphous alloy catalyst after stirring, filtering and drying the filter cake; specifically, filter the suspension obtained by the reaction, stir the filter cake with 400 ml of deionized water and filter it, repeat 3 times, then stir with 400 ml of ethanol and filter it, repeat 2 times to obtain a black filter cake, and vacuum dry the filter cake at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0039] The nickel salt is any one of nickel nitrate, nickel sulfate, nickel acetate and nickel chloride, and the molybdate includes ammonium heptamolybdate or sodium molybdate.

[0040] A supported nickel-based amorphous alloy catalyst is prepared by adopting the above-mentioned preparation method, and the supported nickel-based amorphous alloy catalyst is Ni-Mo-P / SiO2.

[0041] The invention discloses an application of a supported nickel-based amorphous alloy catalyst, wherein the supported nickel-based amorphous alloy catalyst is applied to catalytic hydrogenation of castor oil to synthesize hydrogenated castor oil.

[0042] The method for synthesizing hydrogenated castor oil by catalytic hydrogenation of castor oil comprises the following steps: adding castor oil and a catalyst into a high-pressure autoclave, venting and replacing, adjusting the speed of the autoclave, injecting hydrogen after heating to react, removing hydrogen after the reaction, cooling, and obtaining hydrogenated castor oil; wherein, the venting pressure is 0.01MPa, the speed of the autoclave is 800r / min-1200r / min, the heating temperature is 140℃-180℃, and the reaction time is 0.8h-1.2h.

[0043] Examples: sodium hypophosphite monohydrate (NaH2PO2·H2O), nickel chloride hexahydrate (NiCl2·6H2O), silicon dioxide (SiO2), sodium borohydride (NaBH4), alcohol, ammonium molybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O), sodium acetate (CH3COONa) The above drugs were collected from Sinopharm Group with analytical purity; castor oil, produced by Maclean; distilled water (homemade).

[0044] Example 1

[0045] Preparation of Ni-Mo-P / SiO2: Weigh NiCl2·6H2O (8.10 g, 0.03 mol), (NH4)6Mo7O 24 ·4H2O (0.06g, 0.05mmol) and CH3COONa (1.40g, 0.02mol) were added into 240ml distilled water in a 500ml beaker to dissolve to obtain solution A; NaH2PO2·H2O (3.62g, 0.03mol) was weighed and added into 7ml distilled water in a 50ml beaker to dissolve to obtain solution B; SiO2 (10g) was weighed into a 500ml three-necked flask; solution A and solution B were poured into the three-necked flask containing SiO2 and stirred vigorously, and 0.1ml of 2mol / L NaBH4 solution (as initiator) was slowly added dropwise under nitrogen atmosphere until no bubbles were generated in the solution, indicating that the reaction was over. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0046] Example 2

[0047] Preparation of Ni-Mo-P / SiO2: Weigh NiSO4·6H2O (7.89 g, 0.03 mol), (NH4)6Mo7O 24·4H2O (0.06g, 0.05mmol) and CH3COONa (1.40g, 0.02mol) were added into 240ml distilled water in a 500ml beaker to dissolve to obtain solution A; NaH2PO2·H2O (3.62g, 0.03mol) was accurately weighed into a 50ml beaker and added into 7ml distilled water to dissolve to obtain solution B; SiO2 (10g) was weighed into a 500ml three-necked flask; solution A and solution B were poured into the three-necked flask containing SiO2 and stirred vigorously, and 0.1ml of 2mol / LNaBH4 solution (as initiator) was slowly added dropwise under nitrogen atmosphere until no bubbles were generated in the solution, indicating that the reaction was over. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0048] Example 3

[0049] Preparation of Ni-Mo-P / SiO2: Weigh Ni(CH3COO)2·6H2O (8.55 g, 0.03 mol), (NH4)6Mo7O 24 ·4H2O (0.12g, 0.10mmol) and CH3COONa (1.40g, 0.02mol) were added into 240ml distilled water in a 500ml beaker to dissolve to obtain solution A; NaH2PO2·H2O (5.30g, 0.05mol) was weighed and added into 7ml distilled water in a 50ml beaker to dissolve to obtain solution B; SiO2 (10g) was weighed into a 500ml three-necked flask; solution A and solution B were poured into the three-necked flask containing SiO2 and stirred vigorously, and 0.1ml of 2mol / L NaBH4 solution (as initiator) was slowly added dropwise under nitrogen atmosphere until no bubbles were generated in the solution, indicating that the reaction was over. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0050] Example 4

[0051] Preparation of Ni-Mo-P / SiO2: Weigh NiCl2·6H2O (11.88 g, 0.05 mol), (NH4)6Mo7O 24·4H2O (0.99g, 0.08mmol) and CH3COONa (1.40g, 0.02mol) were added into 240ml distilled water in a 500ml beaker to dissolve to obtain solution A; NaH2PO2·H2O (5.30g, 0.05mol) was weighed and added into 7ml distilled water in a 50ml beaker to dissolve to obtain solution B; SiO2 (10g) was weighed into a 500ml three-necked flask; solution A and solution B were poured into the three-necked flask containing SiO2 and stirred vigorously, and 0.1ml of 2mol / L NaBH4 solution (as initiator) was slowly added dropwise under nitrogen atmosphere until no bubbles were generated in the solution, indicating that the reaction was over. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0052] Example 5

[0053] Preparation of Ni-Mo-P / SiO2: Weigh NiCl2·6H2O (8.10 g, 0.03 mol), Na2MoO4 (0.04 g, 0.40 mmol), and CH3COONa (1.40 g, 0.02 mol) in a 500 ml beaker, add 240 ml of distilled water to dissolve, and obtain solution A; weigh NaH2PO2·H2O (3.62 g, 0.03 mol) in a 50 ml beaker, add 7 ml of distilled water to dissolve, and obtain solution B; weigh SiO2 (10 g) in a 500 ml three-necked flask; pour solution A and solution B into the three-necked flask containing SiO2 and stir vigorously, slowly add 0.1 ml of 2 mol / L NaBH4 solution (as initiator) under nitrogen atmosphere, and the reaction is completed when no bubbles are generated in the solution. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-Mo-P / SiO2 catalyst.

[0054] Comparative Example 1

[0055] Preparation of Ni-P / SiO2 catalyst: Accurately weigh NiCl2·6H2O (8.0995 g, 0.0341 mol) in a 500 ml beaker, add 240 ml distilled water to dissolve, and obtain solution A; accurately weigh NaH2PO2·H2O (9.0296 g, 0.085 mol) in a 100 ml beaker, add 42.6 ml distilled water to dissolve, and obtain solution B; weigh SiO2 (10 g, 0.1667 mol) in a 500 ml three-necked flask; pour solution A and solution B into the three-necked flask containing SiO2 and stir vigorously, slowly add 0.1 ml of 2 mol / L NaBH4 solution (as initiator) in a nitrogen atmosphere, and the reaction is completed when no bubbles are generated in the solution. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and filtered, and this process was repeated 3 times; the filter cake was stirred with 400 ml of ethanol and filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-P / SiO2 catalyst.

[0056] Comparative Example 2

[0057] Preparation of Ni-B / SiO2 catalyst: Accurately weigh NiCl2·6H2O (8.0995g, 0.0341mol) in a 500ml beaker, add 240ml distilled water to dissolve, and obtain solution A; accurately weigh NaBH4 (3.223g, 0.0852mol) in a 100ml beaker, add 42.9ml distilled water to dissolve, and obtain solution B; weigh SiO2 (10g, 0.1667mol) in a 500ml three-necked flask; pour solution A into the three-necked flask containing SiO2 and stir vigorously, slowly add solution B dropwise under nitrogen atmosphere, and the reaction is completed when no bubbles are generated in the solution. The obtained suspension is filtered, and the filter cake is stirred with 400ml deionized water and filtered, and repeated 3 times; then stirred with 400ml ethanol and filtered, and repeated 2 times; a black filter cake is obtained, and the filter cake is vacuum dried at 85℃ for 2h to obtain Ni-B / SiO2 catalyst.

[0058] Comparative Example 3

[0059] Preparation of Ni-BP / SiO2 catalyst: Accurately weigh NiCl2·6H2O (8.0995 g, 0.0341 mol) in a 500 ml beaker, add 240 ml distilled water to dissolve, and obtain solution A; accurately weigh NaH2PO2·H2O (3.62 g, 0.0341 mol) in a 50 ml beaker, add 7 ml distilled water to dissolve, and obtain solution B; accurately weigh NaBH4 (3.223 g, 0.0852 mol) in a 100 ml beaker, add 42.9 ml distilled water to dissolve, and obtain solution C; weigh SiO2 (10 g, 0.1667 mol) in a 500 ml three-necked flask; pour solution A into the three-necked flask containing SiO2 and stir vigorously, slowly add solution B and solution C dropwise under a nitrogen atmosphere, and the reaction is completed when no bubbles are generated in the solution. The obtained suspension was filtered, and the filter cake was stirred with 400 ml of deionized water and then filtered, and this process was repeated 3 times; then, the suspension was stirred with 400 ml of ethanol and then filtered, and this process was repeated 2 times; a black filter cake was obtained, and the filter cake was vacuum dried at 85°C for 2 hours to obtain a Ni-BP / SiO2 catalyst.

[0060] Test and Inspection

[0061] The amorphous alloy catalysts prepared in Examples 1-5 and Comparative Examples 1-3 were respectively tested for their activity in catalytic hydrogenation of castor oil to synthesize hydrogenated castor. For the hydrogenation reaction of castor oil, the hydroxyl value is the main indicator for evaluating the selectivity of the catalyst, and the iodine value is the main indicator for evaluating the activity of the catalyst.

[0062] The specific test method is as follows:

[0063] Example 1: Catalyst Ni-Mo-P / SiO2 activity test: Figure 3 As shown, 100g castor oil and 2g Ni-Mo-P / SiO2 catalyst are added to a 500mL autoclave 5 (a heating jacket is provided in the autoclave 5, a fixture 3 is provided at the top of the autoclave 5, and a thermocouple 4 is also provided inside the autoclave), and the autoclave is emptied to 0.01MPa and replaced three times (the air is evacuated through the N2 in the N2 bottle 1). The speed of the reactor is adjusted to 1000r / min, and after heating to 160°C, hydrogen gas 2MPa is injected through the H2 bottle 2, and the reaction is stopped after 1h. After the reaction is completed, the hydrogen in the reaction system is vacuum-removed, cooled to room temperature, and the product is taken out. The iodine value and hydroxyl value of the product are measured, and the iodine value is 2.77g / 100g and the hydroxyl value is 159.90mg / g.

[0064] Example 2: Activity test of catalyst Ni-Mo-P / SiO2: 100g castor oil and 2g Ni-Mo-P / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected into the reactor at 2MPa after the temperature was raised to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 5.17g / 100g and the hydroxyl value was 153.47mg / g.

[0065] Example 3: Activity test of catalyst Ni-Mo-P / SiO2: 100g castor oil and 2g Ni-Mo-P / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected into the reactor at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 6.47g / 100g and the hydroxyl value was 156.87mg / g.

[0066] Example 4: Activity test of catalyst Ni-Mo-P / SiO2: 100g castor oil and 2g Ni-Mo-P / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 3.32g / 100g and the hydroxyl value was 157.29mg / g.

[0067] Example 5: Activity test of catalyst Ni-Mo-P / SiO2: 100g castor oil and 2g Ni-Mo-P / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 4.85g / 100g and the hydroxyl value was 151.57mg / g.

[0068] Comparative Example 1: Activity test of catalyst Ni-P / SiO2: 100g castor oil and 4g Ni-P / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected into the reactor at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 42.56mg / g and the hydroxyl value was 157.23mg / g.

[0069] Comparative Example 2: Activity test of catalyst Ni-B / SiO2: 100g castor oil and 4g Ni-B / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected into the reactor at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 12.54g / 100g and the hydroxyl value was 155.51mg / g.

[0070] Comparative Example 3: Activity test of catalyst Ni-BP / SiO2: 100g castor oil and 2g Ni-BP / SiO2 catalyst were added to a 500mL autoclave, vented to 0.01MPa and replaced three times. The speed of the reactor was adjusted to 1000r / min, and hydrogen was injected into the reactor at 2MPa after heating to 160°C. The reaction was stopped after 1h. After the reaction was completed, the hydrogen in the reaction system was removed by vacuum, cooled to room temperature, and the product was taken out. The iodine value and hydroxyl value of the product were measured, and the iodine value was 5.76g / 100g and the hydroxyl value was 157.90mg / g.

[0071] In summary, among the series of amorphous alloy catalysts of the present invention, the Ni-Mo-P / SiO2 amorphous alloy catalyst has the best catalytic activity and catalytic selectivity for the selective hydrogenation reaction of castor oil. Figure 5 (a) is the SEM image of the carrier SiO2, from which it can be seen that the carrier is an irregular block structure; Figure 5 (b) is the SEM image of Ni-P / SiO2, which shows spherical particles with good dispersion and no obvious agglomeration. The catalyst particle size is between 120nm and 200nm. Figure 5 (c) It can be seen that the Ni-B / SiO2 amorphous alloy catalyst is irregular in shape, well dispersed, slightly agglomerated, and the catalyst particle size is 60nm-120nm; Figure 5 (d) Figure 5It can be seen from (e) that the Ni-BP / SiO2 and Ni-Mo-P / SiO2 amorphous alloy catalysts are approximately spherical particles with good dispersion. The catalyst particle size is between 40nm and 80nm, and Ni-Mo-P is more evenly dispersed on the carrier, indicating that the addition of Mo further improves the disorder and dispersion of Ni in the catalytic active sites.

[0072] The properties of the Ni-Mo-P / SiO2 amorphous alloy catalyst prepared by the present invention are shown in the figure below: Figure 4 The present invention is the first to use Ni-Mo-P / SiO2 amorphous alloy catalyst in the oil hydrogenation process. The hydrogenated castor oil product produced under the action of the catalyst is milky white (such as Figure 6 The product purity is 84.06% (as shown in Table 1 and Figure 7 As shown). The various quality indicators of hydrogenated castor oil products prepared under the action of Ni-Mo-P / SiO2 catalyst with nickel chloride as nickel source all meet the national standards (iodine value ≤ 5.0g / 100g; hydroxyl value 150-165mg / g), and the catalyst service life is up to 100h. At the same time, the Ni-Mo-P / SiO2 catalyst can be prepared by a simple impregnation-chemical reduction method and can be used for industrial scale-up production. Table 1 is a chemical composition table of hydrogenated castor oil.

[0073] Table 1: Chemical composition of hydrogenated castor oil

[0074]

[0075]

[0076] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a supported nickel-based amorphous alloy catalyst, characterized in that: The following steps are involved: Add water to dissolve nickel salt, molybdate and sodium acetate to obtain solution A; Add water to dissolve sodium hypophosphite monohydrate to obtain solution B; Pour solution A and solution B into a container filled with silica and stir, then slowly add sodium borohydride dropwise to react; The suspension obtained by the reaction is filtered, and the filter cake is stirred, filtered and dried to obtain an amorphous alloy catalyst.

2. The method for preparing a supported nickel-based amorphous alloy catalyst according to claim 1, wherein: The amount of the nickel salt added is 0.03 mol-0.05 mol, the amount of the molybdate added is 0.05 mmol-0.40 mmol, and the amount of the sodium acetate added is 0.01 mol-0.03 mol.

3. The method for preparing a supported nickel-based amorphous alloy catalyst according to claim 1 or 2, wherein: The nickel salt is any one of nickel nitrate, nickel sulfate, nickel acetate and nickel chloride, and the molybdate includes ammonium heptamolybdate or sodium molybdate.

4. The method for preparing a supported nickel-based amorphous alloy catalyst according to claim 1, wherein: The added amount of the sodium hypophosphite monohydrate is 0.03 mol-0.05 mol.

5. The method for preparing a supported nickel-based amorphous alloy catalyst according to claim 1, wherein: The sodium borohydride was added dropwise under a nitrogen atmosphere, with an addition amount of 0.1 ml and a concentration of 2 mol / L.

6. The method for preparing a supported nickel-based amorphous alloy catalyst according to claim 1, wherein: The filter cake obtained after the suspension is filtered is stirred with water and filtered, and then stirred with ethanol and filtered, and then dried to obtain an amorphous alloy catalyst.

7. A supported nickel-based amorphous alloy catalyst, characterized in that: The catalyst is prepared by the preparation method according to any one of claims 1 to 6, wherein the supported nickel-based amorphous alloy catalyst is Ni-Mo-P / SiO2.

8. Use of a supported nickel-based amorphous alloy catalyst according to claim 7, characterized in that: Supported nickel-based amorphous alloy catalyst was used for the catalytic hydrogenation of castor oil to synthesize hydrogenated castor oil.

9. The use of a supported nickel-based amorphous alloy catalyst according to claim 8, characterized in that: The method for synthesizing hydrogenated castor oil by catalytic hydrogenation of castor oil comprises the following steps: adding castor oil and a catalyst into an autoclave, venting and replacing the autoclave, adjusting the speed of the autoclave, heating the autoclave, injecting hydrogen to carry out reaction, removing hydrogen after the reaction is completed, and cooling the autoclave to obtain hydrogenated castor oil.

10. The use of a supported nickel-based amorphous alloy catalyst according to claim 9, characterized in that: The venting pressure is 0.01 MPa, the rotation speed of the reactor is 800 r / min-1200 r / min, the heating temperature is 140° C.-180° C., and the reaction time is 0.8 h-1.2 h.

Citation Information

Cited By

  • Catalyst for hydrogenation dearomatization of waste lubricating oil and preparation method thereof

    CN120662384A

  • A catalyst for hydrodearomatization of waste lubricating oil and a method for preparing the same

    CN120662384B