Manganese-based air purification material and preparation method thereof
Through the synergistic action of modified graphene oxide and nanomanganese dioxide, the characteristics of polydopamine and polyetheramine are used to form manganese-based air purification materials, solving the problems of low catalytic efficiency and high temperature, and achieving efficient formaldehyde purification effect , and maintain high-efficiency catalytic performance in visible light for a long time.
Patent Information
- Application Number
- CN202411142318.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The existing catalytic oxidation materials such as manganese dioxide have problems with low catalytic efficiency and high temperature when catalyzing formaldehyde, and the photocatalytic efficiency and poor stability under visible light.
Polydopamine is self-polymerized by dopamine hydrochloride to form polydopamine. By modifying graphene oxide and nanomanganese dioxide under suitable conditions, a manganese-based air purification material is formed, and the catalytic activity is improved by using the super adhesion properties and thermal conductivity of polydopamine. The three-dimensional framework structure is formed through the molecular link branches of polyetheramine, which enhances the adsorption and catalytic capacity of nanomanganese dioxide.
Excellent purification efficiency of formaldehyde (greater than 90%) is achieved at room temperature, and efficient catalytic performance is maintained for a long time under visible light conditions, avoiding secondary contamination.
Smart Images

Figure BDA0005001212630000091 
Figure BDA0005001212630000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of air purification, and in particular to a manganese-based air purification material and a preparation method thereof. Background Art
[0002] Indoor formaldehyde and other harmful substances mainly come from furniture, flooring, paint and other decoration materials, especially the adhesives used in artificial boards. Some often overlooked items such as curtains, carpets, wallpaper and decorations can also release formaldehyde.
[0003] Commonly used methods for treating indoor formaldehyde include ventilation, green plants, activated carbon, photocatalysts, catalytic oxidation, etc.
[0004] Although ventilation and green plants cost the least, they are inefficient and have a long cycle.
[0005] Activated carbon has a high specific surface area and pore volume, and can effectively adsorb formaldehyde molecules inside the pores through van der Waals forces. However, when the physically adsorbed formaldehyde is saturated, desorption will occur, leading to secondary pollution. Therefore, it is short-lived and needs to be replaced regularly.
[0006] The degradation mechanism of formaldehyde by photocatalyst materials such as titanium dioxide is mainly based on their photocatalytic activity. Under light conditions, they can degrade organic pollutants such as formaldehyde into harmless carbon dioxide and water or other inorganic small molecules. However, photocatalyst materials have certain requirements for the response wavelength of light. The photocatalytic activity of titanium dioxide is mainly in the ultraviolet light region. This is because its band gap width is about 3.2eV, which corresponds to a wavelength of ultraviolet light of about 380nm. Therefore, it faces problems such as low photocatalytic efficiency under visible light and poor stability of photocatalyst materials.
[0007] Catalytic materials such as manganese dioxide mainly promote the adsorption and activation of formaldehyde molecules by forming active sites on the catalyst surface, which then react with oxygen to produce carbon dioxide and water. Due to their high catalytic activity, thermal stability, low cost and availability of various crystal forms, they have attracted much attention in the study of catalytic oxidation of formaldehyde in the air. However, there are still problems with high catalytic temperature (above 50°C) and low catalytic efficiency. Summary of the invention
[0008] In order to overcome the defects of the prior art, a manganese-based air purification material and a preparation method thereof are provided to solve the problem of low catalytic efficiency of existing catalytic oxidation materials such as manganese dioxide used for formaldehyde treatment.
[0009] To achieve the above object, a method for preparing a manganese-based air purification material is provided, comprising the following steps:
[0010] adding graphene oxide to a dopamine hydrochloride solution, and stirring the reaction under heating reflux conditions to obtain a polydopamine-modified graphene oxide dispersion;
[0011] grinding nano manganese dioxide and a dispersant in a grinding liquid to obtain a modified nano manganese dioxide dispersion;
[0012] The polydopamine-modified graphene oxide dispersion and the polyetheramine are added to the modified nano manganese dioxide dispersion respectively, and stirred to react under heating reflux conditions. After the reaction, the manganese-based air purification material is obtained by sequentially filtering, washing and freeze-drying.
[0013] Furthermore, the dopamine hydrochloride solution is obtained by dissolving dopamine hydrochloride in a Tris-HCl buffer solution, and the pH value of the Tris-HCl buffer solution is 8-10.
[0014] Furthermore, the diameter of the graphene oxide flakes is 5 to 10 microns.
[0015] Furthermore, the content of polydopamine-modified graphene oxide in the polydopamine-modified graphene oxide dispersion is 5 to 10 mg / mL.
[0016] Furthermore, the mass ratio of the dopamine hydrochloride to the graphene oxide is 1:2 to 1:1.
[0017] Furthermore, the dispersant is at least one of polyvinyl pyrrolidone, polyethylene imine, and ammonium polyacrylate.
[0018] Furthermore, the particle size of the nano manganese dioxide is 20 to 50 nm.
[0019] Furthermore, the modified nano-manganese dioxide content in the modified nano-manganese dioxide dispersion is 30-50 mg / mL, and the mass fraction of the dispersant is 1-2 wt %.
[0020] Furthermore, the mass ratio of polydopamine-modified graphene oxide, modified nano manganese dioxide and polyetheramine in the polydopamine-modified graphene oxide / modified nano manganese dioxide / polyetheramine composite is (1-2): (2-4): (2-3).
[0021] The present invention provides a manganese-based air purification material, which is prepared by adopting the above-mentioned preparation method of manganese-based air purification material.
[0022] The beneficial effects of the present invention are:
[0023] The manganese-based air purification material of the present invention uses dopamine hydrochloride to self-polymerize to generate polydopamine, wherein the polydopamine has super strong adhesion performance and can simultaneously reduce and surface-modify graphene oxide. On the one hand, the reduction of polydopamine improves the thermal conductivity and photothermal effect of graphene oxide. Under light conditions, the heat generated by the reduction of graphene oxide and polydopamine can be quickly transferred to nano manganese dioxide particles, thereby activating the lattice oxygen on the surface of manganese dioxide and accelerating the catalytic oxidation degradation of formaldehyde. On the other hand, the surface modification of polydopamine can not only hinder the agglomeration of reduced graphene oxide in the aqueous reaction solution and increase the adsorption area of nano-manganese dioxide particles and formaldehyde molecules, but also its adhesion performance provides sites for the attachment of nano-manganese dioxide particles to the surface of reduced graphene oxide nanosheets, which helps to evenly disperse the nano-manganese dioxide particles on the reduced graphene oxide nanosheets. The interfacial hybridization between the nano-manganese dioxide particles and the reduced graphene oxide nanosheets is conducive to electron transmission, increases the surface charge density of the nano-manganese dioxide particles, and promotes the activation of oxygen molecules, thereby enhancing the catalytic activity of manganese dioxide, and has excellent formaldehyde purification efficiency (greater than 90%) at room temperature.
[0024] The manganese-based air purification material of the present invention has nano manganese dioxide which has abundant unsaturated electron holes and can activate oxygen and water in the air to generate active oxygen and active hydroxyl groups, thereby decomposing formaldehyde into water and carbon dioxide.
[0025] In the present invention, the dispersant and the grinder are used for surface modification of nano manganese dioxide particles, promoting their dispersion in the aqueous reaction solution and uniform particle size, so as to better adsorb to the surface of the reduced graphene oxide nanosheets.
[0026] In the present invention, the polyetheramine contains terminal amine groups at both ends of the molecular chain. Under suitable reaction conditions, not only can the residual oxygen-containing functional groups on the surface of the polydopamine-reduced graphene oxide be further reduced to improve the thermal conductivity and photothermal efficiency of the reduced graphene oxide, but also the two ends of the molecular chain can be respectively grafted to the surfaces of adjacent reduced graphene oxide nanosheets, so that the reduced graphene oxide nanosheets loaded with nano manganese dioxide particles are bridged to each other, thereby forming a three-dimensional framework structure, and the structure can be retained after freeze-drying, thereby enhancing the adsorption and catalytic oxidation degradation of formaldehyde in the air. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.
[0028] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below in conjunction with the embodiments.
[0029] The present invention provides a method for preparing a manganese-based air purification material, comprising the following steps:
[0030] S1. Adding graphene oxide to a dopamine hydrochloride solution, and stirring the reaction under heating reflux conditions to obtain a polydopamine-modified graphene oxide dispersion.
[0031] In this embodiment, the dopamine hydrochloride solution is obtained by dissolving dopamine hydrochloride in a Tris-HCl buffer solution. The Tris-HCl buffer solution provides an alkaline environment for the self-polymerization reaction of dopamine hydrochloride. Further, the pH value is preferably 8-10.
[0032] In this embodiment, the diameter of the graphene oxide sheet is 5 to 10 micrometers.
[0033] In this embodiment, the content of polydopamine-modified graphene oxide in the polydopamine-modified graphene oxide dispersion is 5 to 10 mg / mL.
[0034] In this embodiment, the mass ratio of dopamine hydrochloride to graphene oxide is 1:2 to 1:1.
[0035] In step S1, the heating temperature for the self-polymerization reaction of dopamine hydrochloride on the surface of graphene oxide is preferably 45-60° C., the stirring speed is preferably 300-500 rpm, and the reaction time is preferably 4-5 h.
[0036] S2. Grinding the nano manganese dioxide and the dispersant in a grinding liquid to obtain a modified nano manganese dioxide dispersion.
[0037] In this embodiment, the dispersant is at least one of polyvinyl pyrrolidone, polyethylene imine, and ammonium polyacrylate.
[0038] In this embodiment, the particle size of nano manganese dioxide is 20-50 nm.
[0039] In this embodiment, the content of modified nano-manganese dioxide in the modified nano-manganese dioxide dispersion is 30-50 mg / mL, and the mass fraction of the dispersant is 1-2 wt %.
[0040] Specifically, the grinding is performed using a grinder, which is preferably at least one of a ball mill and a sand mill, with a grinding speed of preferably 400 to 800 rpm and a grinding time of preferably 3 to 5 hours.
[0041] S3. Adding the polydopamine-modified graphene oxide dispersion and the polyetheramine into the modified nano manganese dioxide dispersion respectively, and stirring the mixture under heating reflux conditions to react, and after the reaction, filtering, washing, and freeze-drying the mixture in sequence to obtain a manganese-based air purification material.
[0042] In this embodiment, the mass ratio of polydopamine-modified graphene oxide, modified nano manganese dioxide and polyetheramine in the polydopamine-modified graphene oxide / modified nano manganese dioxide / polyetheramine composite is (1-2): (2-4): (2-3).
[0043] In this embodiment, the number average molecular weight of the polyetheramine is preferably 230-2000 g / mol.
[0044] In step S3, the heating temperature of the heating reflux condition is preferably 75 to 90°C, the stirring speed is preferably 600 to 800 rpm, the reaction time is preferably 8 to 12 hours, and the freeze-drying time is preferably 12 to 24 hours.
[0045] The present invention provides a manganese-based air purification material, which is prepared by adopting the above-mentioned preparation method of manganese-based air purification material.
[0046] The manganese-based air purification material of the present invention uses dopamine hydrochloride to self-polymerize to generate polydopamine, wherein the polydopamine has super strong adhesion performance and can simultaneously reduce and surface-modify graphene oxide. On the one hand, the reduction of polydopamine improves the thermal conductivity and photothermal effect of graphene oxide. Under light conditions, the heat generated by the reduction of graphene oxide and polydopamine can be quickly transferred to nano manganese dioxide particles, thereby activating the lattice oxygen on the surface of manganese dioxide and accelerating the catalytic oxidation degradation of formaldehyde. On the other hand, the surface modification of polydopamine can not only hinder the agglomeration of reduced graphene oxide in the aqueous reaction solution and increase the adsorption area of nano-manganese dioxide particles and formaldehyde molecules, but also its adhesion performance provides sites for the attachment of nano-manganese dioxide particles to the surface of reduced graphene oxide nanosheets, which helps to evenly disperse the nano-manganese dioxide particles on the reduced graphene oxide nanosheets. The interfacial hybridization between nano-manganese dioxide particles and reduced graphene oxide nanosheets is conducive to electron transmission, increases the surface charge density of nano-manganese dioxide particles, and promotes the activation of oxygen molecules, thereby enhancing the catalytic activity of manganese dioxide, and has excellent formaldehyde purification efficiency at room temperature.
[0047] The manganese-based air purification material of the present invention has nano manganese dioxide which has abundant unsaturated electron holes and can activate oxygen and water in the air to generate active oxygen and active hydroxyl groups, thereby decomposing formaldehyde into water and carbon dioxide.
[0048] In the present invention, the dispersant and the grinder are used for surface modification of nano manganese dioxide particles, promoting their dispersion in the aqueous reaction solution and uniform particle size, so as to better adsorb to the surface of the reduced graphene oxide nanosheets.
[0049] In the present invention, the polyetheramine contains terminal amine groups at both ends of the molecular chain. Under suitable reaction conditions, not only can the residual oxygen-containing functional groups on the surface of the polydopamine-reduced graphene oxide be further reduced to improve the thermal conductivity and photothermal efficiency of the reduced graphene oxide, but also the two ends of the molecular chain can be respectively grafted to the surfaces of adjacent reduced graphene oxide nanosheets, so that the reduced graphene oxide nanosheets loaded with nano manganese dioxide particles are bridged to each other, thereby forming a three-dimensional framework structure, and the structure can be retained after freeze-drying, thereby enhancing the adsorption and catalytic oxidation degradation of formaldehyde in the air.
[0050] In order to specifically illustrate the manganese-based air purification material and the preparation method thereof of the present invention, the following examples and comparative examples are given for detailed description.
[0051] Example 1
[0052] In this example, manganese-based air purification material I is prepared by the following scheme.
[0053] S1. Dissolve dopamine hydrochloride (Adamas, RG grade) in Tris-HCl buffer solution (self-prepared, pH=8.5), then add graphene oxide (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., flake diameter 10 microns), stir and react under heating reflux conditions (heating temperature 60°C, stirring speed 400rpm, reaction time 5h) to obtain a polydopamine-modified graphene oxide dispersion (polydopamine-modified graphene oxide content is 5 mg / mL, and the mass ratio of dopamine hydrochloride to graphene oxide is 1:1);
[0054] S2, adding dispersant (polyethyleneimine, Adamas, weight average molecular weight ~600g / mol) and nano manganese dioxide (Guangzhou Metallurgical Industry Co., Ltd., 20nm) to deionized water, preparing grinding liquid, grinding in a grinder (ball mill, speed 400rpm, grinding time 5h), to obtain modified nano manganese dioxide dispersion (dispersant mass fraction is 1.5wt%, modified nano manganese dioxide content is 40mg / mL);
[0055] S3. Add the modified nano manganese dioxide dispersion and polyetheramine (Adamas D-400, average number average molecular weight ~400) obtained in S2 to the polydopamine modified graphene oxide dispersion obtained in S1, stir and react under heating reflux conditions (heating temperature 80°C, stirring speed 700rpm, reaction time 10h), let stand and cool, and then repeatedly filter and wash with deionized water, and finally freeze-dry (drying time 24h) to obtain polydopamine modified graphene oxide / modified nano manganese dioxide / polyetheramine composite I (the mass ratio of polydopamine modified graphene oxide, modified nano manganese dioxide and polyetheramine is 1.5:2:2.5).
[0056] Example 2
[0057] In this example, manganese-based air purification material II is prepared by the following scheme.
[0058] S1. Dissolve dopamine hydrochloride (Adamas, RG grade) in Tris-HCl buffer solution (self-prepared, pH=10), then add graphene oxide (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., flake diameter 5 μm), stir and react under heating reflux conditions (heating temperature 50°C, stirring speed 300 rpm, reaction time 4 h) to obtain a polydopamine-modified graphene oxide dispersion (polydopamine-modified graphene oxide content of 10 mg / mL, mass ratio of dopamine hydrochloride to graphene oxide of 1:2);
[0059] S2, adding a dispersant (polyvinyl pyrrolidone (Adamas, K30) and ammonium polyacrylate (Adamas, 40% aqueous solution) in a mass ratio of 1:1) and nano manganese dioxide (Guangzhou Metallurgical Industry Co., Ltd., 50 nm) to deionized water, preparing a grinding liquid, and grinding the mixture in a grinder (sand mill, rotation speed 600 rpm, grinding time 4 h) to obtain a modified nano manganese dioxide dispersion (dispersant mass fraction 1wt%, modified nano manganese dioxide content 50 mg / mL);
[0060] S3. Add the modified nano manganese dioxide dispersion and polyetheramine (Adamas D-230, average number average molecular weight ~230) obtained in S2 to the polydopamine-modified graphene oxide dispersion obtained in S1, stir and react under heating reflux conditions (heating temperature 90°C, stirring speed 800rpm, reaction time 8h), let stand and cool, and then repeatedly filter and wash with deionized water, and finally freeze-dry (drying time 12h) to obtain polydopamine-modified graphene oxide / modified nano manganese dioxide / polyetheramine complex II (the mass ratio of polydopamine-modified graphene oxide, modified nano manganese dioxide and polyetheramine is 2:4:3).
[0061] Example 3
[0062] In this example, manganese-based air purification material III is prepared by the following scheme.
[0063] S1. Dissolve dopamine hydrochloride (Adamas, RG grade) in Tris-HCl buffer solution (self-prepared, pH=8), then add graphene oxide (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., flake diameter 5 μm), stir and react under heating reflux conditions (heating temperature 45°C, stirring speed 500 rpm, reaction time 6 h) to obtain a polydopamine-modified graphene oxide dispersion (polydopamine-modified graphene oxide content of 15 mg / mL, mass ratio of dopamine hydrochloride to graphene oxide of 1:1.5), and set aside;
[0064] S2, adding dispersant (polyvinyl pyrrolidone, Adamas, K17) and nano manganese dioxide (BROFOS, 30 nm) to deionized water, preparing grinding liquid, grinding in a grinder (sand mill, speed 800 rpm, grinding time 3 h), to obtain modified nano manganese dioxide dispersion (dispersant mass fraction is 2 wt%, modified nano manganese dioxide content is 30 mg / mL), and set aside;
[0065] S3. Add the modified nano manganese dioxide dispersion and polyetheramine (Adamas D-2000, average number average molecular weight ~2000) obtained in S2 to the polydopamine modified graphene oxide dispersion obtained in S1, stir and react under heating reflux conditions (heating temperature 75°C, stirring speed 600rpm, reaction time 12h), let stand and cool, and then repeatedly filter and wash with deionized water, and finally freeze-dry (drying time 15h) to obtain polydopamine modified graphene oxide / modified nano manganese dioxide / polyetheramine complex III (the mass ratio of polydopamine modified graphene oxide, modified nano manganese dioxide and polyetheramine is 1:2:2).
[0066] Comparative Example 1
[0067] In this comparative example, a manganese-based air purification material without polydopamine was prepared by the following scheme.
[0068] S1. Add graphene oxide (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., flake diameter 10 μm) into deionized water and perform ultrasonic treatment (40 kHz, 30 min) to obtain a graphene oxide dispersion with a graphene oxide content of 5 mg / mL.
[0069] S2, adding dispersant (polyethyleneimine, Adamas, weight average molecular weight ~600g / mol) and nano manganese dioxide (Guangzhou Metallurgical Industry Co., Ltd., 20nm) to deionized water, preparing grinding liquid, grinding in a grinder (ball mill, speed 400rpm, grinding time 5h), to obtain modified nano manganese dioxide dispersion (dispersant mass fraction is 1.5wt%, modified nano manganese dioxide content is 40mg / mL);
[0070] S3. Add the modified nano manganese dioxide dispersion and polyetheramine (Adamas D-400, average number average molecular weight ~400) obtained in S2 to the graphene oxide dispersion obtained in S1, stir and react under heating reflux conditions (heating temperature 80°C, stirring speed 700rpm, reaction time 10h), let stand and cool, and then repeatedly filter and wash with deionized water, and finally freeze-dry (drying time 24h) to obtain a graphene oxide / modified nano manganese dioxide / polyetheramine composite (the mass ratio of graphene oxide, modified nano manganese dioxide and polyetheramine is 1.5:2:2.5).
[0071] Comparative Example 2
[0072] This comparative example does not contain a manganese-based air purification material containing graphene oxide through the following scheme.
[0073] S1. Dissolve dopamine hydrochloride (Adamas, RG grade) in Tris-HCl buffer solution (self-prepared, pH=8.5), and then stir the reaction under heating reflux conditions (heating temperature 60°C, stirring speed 400 rpm, reaction time 5 h) to obtain a polydopamine dispersion (polydopamine content 10 mg / mL);
[0074] S2, adding dispersant (polyethyleneimine, Adamas, weight average molecular weight ~600g / mol) and nano manganese dioxide (Guangzhou Metallurgical Industry Co., Ltd., 20nm) to deionized water, preparing grinding liquid, grinding in a grinder (ball mill, speed 400rpm, grinding time 5h), to obtain modified nano manganese dioxide dispersion (dispersant mass fraction is 1.5wt%, modified nano manganese dioxide content is 40mg / mL);
[0075] S3. Add the modified nano manganese dioxide dispersion and polyetheramine (Adamas D-400, average number average molecular weight ~400) obtained in S2 to the polydopamine dispersion obtained in S1, stir and react under heating reflux conditions (heating temperature 80°C, stirring speed 700rpm, reaction time 10h), let stand and cool, and then repeatedly filter and wash with deionized water, and finally freeze-dry (drying time 24h) to obtain a polydopamine / modified nano manganese dioxide / polyetheramine complex (the mass ratio of polydopamine, modified nano manganese dioxide and polyetheramine is 2:2.5:2).
[0076] Comparative Example 3
[0077] In this comparative example, a manganese-based air purification material without polyetheramine cross-linking is prepared by the following scheme.
[0078] S1. Dissolve dopamine hydrochloride (Adamas, RG grade) in Tris-HCl buffer solution (self-prepared, pH=8.5), then add graphene oxide (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., flake diameter 10 microns), stir and react under heating reflux conditions (heating temperature 60°C, stirring speed 400rpm, reaction time 5h) to obtain a polydopamine-modified graphene oxide dispersion (polydopamine-modified graphene oxide content is 5 mg / mL, and the mass ratio of dopamine hydrochloride to graphene oxide is 1:1);
[0079] S2, adding dispersant (polyethyleneimine, Adamas, weight average molecular weight ~600g / mol) and nano manganese dioxide (Guangzhou Metallurgical Industry Co., Ltd., 20nm) to deionized water, preparing grinding liquid, grinding in a grinder (ball mill, speed 400rpm, grinding time 5h), to obtain modified nano manganese dioxide dispersion (dispersant mass fraction is 1.5wt%, modified nano manganese dioxide content is 40mg / mL);
[0080] S3. Add the modified nano manganese dioxide dispersion obtained in S2 to the polydopamine-modified graphene oxide dispersion obtained in S1, and after sufficient stirring (stirring speed 700 rpm, stirring time 30 min), repeatedly filter and wash with deionized water, and finally dry (temperature 70°C, drying time 24 h) to obtain a polydopamine-modified graphene oxide / modified nano manganese dioxide composite (the mass ratio of polydopamine-modified graphene oxide and modified nano manganese dioxide is 1.5:2).
[0081] Comparative Example 4
[0082] This comparative example directly uses nano manganese dioxide without any modification as the comparative example sample.
[0083] Comparative Example 5
[0084] This comparative example directly uses activated carbon without any modification as the comparative example sample.
[0085] In the above specific example, the prepared air purification material is prepared according to the powder inorganic coating material (Class 1F) in the standard "JC / T 1074-2021 Purification Performance of Indoor Air Purification Functional Coating Materials" for test samples, and formaldehyde is selected as the target pollutant. The purification principle is based on the photocatalytic air purification function coating material (Type G, visible light source) for performance testing.
[0086] The test results of the corresponding properties of the products formed in Examples 1 to 3 and the products formed in Comparative Examples 1 to 5 are as follows:
[0087]
[0088]
[0089] From the results of the above tests, it can be seen that under the synergistic effect of polydopamine, graphene oxide, polyetheramine and nano manganese dioxide, the prepared manganese-based air purification material has excellent formaldehyde purification efficiency and purification durability under visible light and room temperature conditions compared with manganese-based air purification materials without polydopamine, manganese-based air purification materials without graphene oxide, manganese-based air purification materials not cross-linked by polyetheramine, and pure nano manganese dioxide and activated carbon.
[0090] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.
Claims
1. A method for preparing a manganese-based air purification material, characterized in that: The following steps are involved: adding graphene oxide to a dopamine hydrochloride solution, and stirring the reaction under heating reflux conditions to obtain a polydopamine-modified graphene oxide dispersion; grinding nano manganese dioxide and a dispersant in a grinding liquid to obtain a modified nano manganese dioxide dispersion; The polydopamine-modified graphene oxide dispersion and the polyetheramine are added to the modified nano manganese dioxide dispersion respectively, and stirred to react under heating reflux conditions. After the reaction, the manganese-based air purification material is obtained by sequentially filtering, washing and freeze-drying.
2. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The dopamine hydrochloride solution is obtained by dissolving dopamine hydrochloride in a Tris-HCl buffer solution, and the pH value of the Tris-HCl buffer solution is 8-10.
3. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The diameter of the graphene oxide sheet is 5 to 10 microns.
4. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The content of polydopamine-modified graphene oxide in the polydopamine-modified graphene oxide dispersion is 5 to 10 mg / mL.
5. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The mass ratio of the dopamine hydrochloride to the graphene oxide is 1:2 to 1:
1.
6. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The dispersant is at least one of polyvinyl pyrrolidone, polyethylene imine and ammonium polyacrylate.
7. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The particle size of the nano manganese dioxide is 20-50 nm.
8. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The modified nano manganese dioxide content in the modified nano manganese dioxide dispersion is 30-50 mg / mL, and the mass fraction of the dispersant is 1-2 wt %.
9. The method for preparing a manganese-based air purification material according to claim 1, characterized in that: The mass ratio of polydopamine-modified graphene oxide / modified nano manganese dioxide / polyetheramine composite is (1-2): (2-4): (2-3).
10. A manganese-based air purification material, characterized in that: The manganese-based air purification material is prepared by the preparation method of the manganese-based air purification material as described in any one of claims 1 to 9.