Shell manufacturing process for preventing large-size directional mold shell from expanding

By wrapping carbon fiber cloth outside the mold shell to reinforce, the problems of low thermal conductivity and mismatch of thermal expansion coefficient are solved, the quality and forming effect of the castings are improved, and the efficient production of large-size hollow directional blades is achieved.

CN119035450APending Publication Date: 2024-11-29ANHUI YINGLIU ELECTROMECHANICAL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411173223.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing single crystal directional die shell technology, the mold shell strength is insufficient, the thermal conductivity is low, and the thermal expansion coefficient is mismatched, resulting in the castings being easily broken or deformed in high temperature and high pressure environments, making it difficult to control the size and shape of the blades.

Method used

The carbon fiber cloth is wrapped in the molded shell and reinforced the mold shell. Through the high strength, heat resistance and low thermal expansion coefficient of the carbon fiber cloth, the strength and heat conduction effect of the mold shell are improved, and the thermal expansion characteristics of the casting are matched to avoid deformation and cracking.

Benefits of technology

It effectively improves the strength and thermal conductivity of the mold shell, uniforms the temperature gradient of the casting, reduces the failure rate and rework rate, improves the quality and forming effect of the casting, and realizes efficient production of large-size hollow directional blades.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a shell manufacturing process for preventing expansion of a large-size directional shell, the shell is a turbine blade shell of a heavy duty gas turbine, the manufacturing process comprises the following steps: pre-preparing shell slurry, preparing a shell manufacturing environment, controlling the number of shell manufacturing layers, dewaxing the shell, pre-roasting the shell after dewaxing is completed, and cutting carbon fiber cloth. After being wetted, the mold shell is wrapped, and after shell manufacturing is completed, the mold shell is cleaned and inspected; the carbon fiber cloth is wrapped outside the mold shell to reinforce the mold shell, so that the strength of the mold shell is improved, the mold shell is prevented from cracking or deforming in the casting process, the heat conduction effect of the mold shell can be improved, the temperature gradient of a casting is more uniform, the thermal stress between the casting and the mold shell can be relieved, and deformation or cracking of the casting is avoided; the problem of mismatching of thermal expansion coefficients is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precision casting, and in particular to a mold shell manufacturing process for preventing large-size directional mold shell from expanding. Background Art

[0002] Oriented single crystal blades are one of the key components in high temperature and high pressure working environments such as aerospace engines and industrial gas turbines. They have strong high temperature resistance, corrosion resistance and tensile resistance, can improve combustion efficiency and reduce weight, and enhance engine reliability and performance.

[0003] The mold shell process technology is one of the key processes for preparing large oriented single crystal blades. The mold shell is the mold shell that wraps the blade during the single crystal growth process, which is used to protect the mold and blade during the single crystal growth process. At the same time, the mold shell can also adjust the solidification rate and temperature gradient during the single crystal growth process by controlling the expansion and contraction of the mold shell, affecting the key properties of the single crystal such as grain boundary clarity, crystal orientation and grain size distribution.

[0004] Heavy-duty gas turbines are the most efficient heat-to-power conversion power generation equipment to date. Their R&D and manufacturing level represents the level of a country's heavy industry, marks the country's technological development, and is also a key equipment in my country's energy development strategy. Turbine blades working in high temperature and complex stress environments are the core hot end components of heavy-duty gas turbines. In order to cope with the extreme service conditions of heavy-duty gas turbines and higher power output, the turbine blades of heavy-duty gas turbines have transitioned to hollow directional columnar crystals or single crystal blades. Compared with aircraft engines, the turbine blades of heavy-duty gas turbines are larger in size, with a length greater than 510mm, a general weight greater than 10kg, and a complex air-cooled inner cavity structure. The manufacturing process difficulty of large-size turbine blades for heavy-duty gas turbines has increased significantly, and the blade size is difficult to control, especially because the blade shell strength does not meet the standard during the manufacturing process. The problem of excessive size caused by the shape is more prominent.

[0005] The disadvantages of existing single crystal oriented shell technology are:

[0006] 1. Insufficient mold shell strength: Due to the limited preparation process of the mold shell, it is often unable to achieve sufficient strength, which can easily cause the mold shell to crack or deform during the casting process.

[0007] 2. Low thermal conductivity: The existing mold shell is often affected by high temperature during the casting process, resulting in uneven heat inside the mold shell and poor heat conduction, which easily leads to uneven temperature gradient of the casting.

[0008] 3. Mismatch in thermal expansion coefficient: The existing mold shell materials often do not match the thermal expansion coefficient of the casting material, which can easily lead to stress concentration between the casting and the mold shell, thereby causing deformation or cracking of the casting.

[0009] To this end, the present application proposes a mold shell manufacturing process that prevents large-sized directional mold shell from expanding, so as to solve the above-mentioned problem. Summary of the invention

[0010] The main purpose of the present invention is to provide a mold shell manufacturing process that prevents large-sized directional mold shells from expanding, which can effectively solve the problems in the background technology.

[0011] In order to solve the above technical problems, the technical solution adopted by the present invention is: a shell manufacturing process for preventing the large-size directional shell from expanding, the shell is a turbine blade shell of a heavy-duty gas turbine, and the manufacturing process includes the following steps:

[0012] 1) Pre-configuration of shell slurry: According to the requirements of shell reinforcement, select appropriate shell slurry components, and configure, mix and prepare slurry according to the selected shell slurry components;

[0013] 2) Preparation of the shell making environment: the shell making temperature is 20-25℃, the humidity is 40-60%, and a robot and an automatic control system are configured;

[0014] 3) Control of the number of shell layers: There are four types of shells, from inside to outside, namely surface layer, transition layer, reinforcement layer and sealing layer;

[0015] 4) Shell dewaxing: Use hot air or steam to heat the shell to melt and discharge the wax core. After dewaxing is completed, pre-bake the shell;

[0016] 5) Shell outer surface treatment: according to the outer surface size of the shell, cut the carbon fiber cloth, wrap it outside the shell after wetting, and dry it naturally for more than 24 hours;

[0017] 6) Cleaning and inspection of the shell: After the shell is made, use high-pressure air to flush the inner cavity to remove residual impurities, use methylene blue solution to detect leakage, and observe whether there is leakage. Finally, use pure water to flush the inner cavity of the shell to clean up the methylene blue solution and other residues.

[0018] Preferably, the medium-sized shell slurry components in step 1) include zircon powder, silica sol, a wetting agent and a defoaming agent.

[0019] Preferably, in the step 3), the material of the surface layer is 100-200 mesh zircon powder, which is used to increase the surface smoothness and hardness of the mold shell; the material of the transition layer is a mixture of 100-200 mesh zircon powder and 70-150 mesh zircon powder of the surface layer, which is used to connect the surface layer and the reinforcement layer; the material of the reinforcement layer is 50-120 mesh zircon powder and mullite particles, which are used to enhance the strength and rigidity of the mold shell; the material of the sealing layer is 100-200 mesh quartz sand, which is used to protect the mold shell and the reinforcement layer.

[0020] Preferably, in step 5), the carbon fiber cloth is immersed in the slurry of the reinforcement layer to wet the carbon fiber cloth, and before the carbon fiber cloth is attached to the shell, the slurry of the reinforcement layer is used to wet the outer surface of the shell, so that the wetted carbon fiber cloth is tightly attached to the shell surface.

[0021] Preferably, the carbon fiber cloth in step 5) is 3K240G twill-shaped carbon fiber cloth.

[0022] Preferably, in step 5), the carbon fiber cloth wrapped around the blade body is divided into three sections according to height and the connection point of the carbon fiber cloth wrapped in the same section is located on the back of the blade, and the tenon of the blade is wrapped with a whole piece of carbon fiber cloth.

[0023] Compared with the traditional technology, the beneficial effects produced by the present invention are as follows: the present invention reinforces the mold shell by wrapping carbon fiber cloth outside the mold shell, utilizes the high strength and heat resistance of the carbon fiber cloth to improve the strength of the mold shell, avoids the mold shell from cracking or deformation during the casting process, and utilizes the good thermal conductivity of the carbon fiber cloth to improve the thermal conduction effect of the mold shell, making the temperature gradient of the casting more uniform; the carbon fiber cloth has a low thermal expansion coefficient, which can alleviate the thermal stress between the casting and the mold shell, avoid deformation or cracking of the casting, and solve the problem of thermal expansion coefficient mismatch; the present invention effectively solves the shortcomings of the existing single crystal directional mold shell technology, improves the strength, thermal conductivity and thermal expansion coefficient matching of the mold shell, thereby improving the quality of the casting and the forming effect.

[0024] The heavy-duty gas large-size hollow directional blade shell prepared by this casting shell making process has a low failure rate, good casting surface integrity, and the blade contour size meets the design standard of the drawing. The contour rework rate of the casting shell making process is low, and the overall rework area of ​​the blade is within 10%, which greatly shortens the rework time and greatly reduces the manufacturing cost of the product. A large-scale production process system for heavy-duty gas turbine blades has been established, reaching the international advanced level in terms of product comprehensive performance, geometric dimensions and overall quality, and realizing mass production and application. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0026] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features and technical solutions in the embodiments may be combined with each other.

[0027] A shell manufacturing process for preventing large-size directional shell from expanding, wherein the shell is a turbine blade shell of a heavy-duty gas turbine, and the manufacturing process comprises the following steps:

[0028] 1) Pre-configuration of shell slurry: First, according to the requirements of shell reinforcement, select the appropriate shell slurry components, usually including zircon powder, silica sol, some wetting agents and defoaming agents. In terms of proportion, it is generally configured according to a certain ratio, and the ratio can be adjusted according to the specific materials used. During pre-configuration, add defoaming agents to remove bubbles in the slurry, and wetting agents to maintain the fluidity of the slurry;

[0029] 2) Preparation of the shell making environment: First, the temperature and humidity need to be controlled. The temperature needs to be kept within an appropriate range, usually between 20-25°C, to ensure that the hardening process of the slurry can proceed normally. In terms of humidity, the relative humidity is generally required to be between 40-60% to avoid premature water loss or excessive wetting of the slurry. In addition, the manipulator and automatic control system need to be prepared to ensure the accuracy and stability of the shell making process;

[0030] 3) Control of the number of shell layers in the mold making process: During the mold making process, the surface layer, transition layer, reinforcement layer and sealing layer are coated on the surface of the wax mold from the inside to the outside. The function of the surface layer is to increase the surface smoothness and hardness of the mold shell. The material used is the finest zircon powder with a particle size of 100-200 mesh. The transition layer is used to connect the surface layer and the reinforcement layer. It is made of a mixture of coarser zircon powder and the surface layer material, specifically a mixture of 100-200 mesh mullite powder and 70-150 mesh mullite powder. The reinforcement layer is the key layer, which enhances the strength and rigidity of the mold shell. The materials used are coarser zircon powder and mullite particles with a particle size of 50-120 mesh. The sealing layer is the outermost layer, which is used to protect the mold shell and the reinforcement layer. The material of the sealing layer is 100-200 mesh quartz sand. It can also be applied with the mold shell slurry as a sealing layer;

[0031] 4) Mold shell dewaxing: Dewaxing means melting and removing the wax core in the mold shell so as to form the inner cavity of the mold shell in the subsequent pre-baking process. Dewaxing uses hot air or steam to heat the mold shell to melt and discharge the wax core. After dewaxing, pre-baking is performed to enhance the strength and stability of the mold shell.

[0032] 5) Shell outer surface treatment:

[0033] After the shell is pre-baked, the carbon fiber cloth is cut according to the outer surface size of the shell. The carbon fiber cloth adopts 3K240G twill shaped carbon fiber cloth so that the carbon fiber cloth can just wrap the shell. Before wrapping the shell, the cut carbon fiber cloth is immersed in the slurry of the reinforcement layer to wet the carbon fiber cloth, so as to better bond with the shell slurry, and before the carbon fiber cloth is attached to the shell, the slurry of the reinforcement layer is used to wet the outer surface of the shell, and the wetted carbon fiber cloth is tightly attached to the shell surface. The carbon fiber cloth wrapped on the blade body is divided into three sections according to the height and the connection point of the carbon fiber cloth wrapping in the same section is located on the back of the blade. The tenon of the blade is wrapped with a whole piece of carbon fiber cloth. After wrapping, it is naturally dried for more than 24 hours.

[0034] 6) Cleaning and inspection of the shell: After the shell is made, the shell needs to be cleaned and inspected. First, use high-pressure air to flush the inner cavity to remove residual wax ash, dust and other impurities to ensure that the inner cavity is clean. Next, use methylene blue solution to perform leakage detection, fill the inner cavity of the shell with methylene blue solution, and observe whether there is leakage to ensure the sealing of the shell. Finally, use pure water to flush the inner cavity to clean the methylene blue solution and other residues to ensure the cleanliness of the inner cavity.

[0035] During pouring, the melting furnace should be heated up slowly and kept warm in stages. When the pouring temperature is reached, the mold shell insulation should be controlled within 30 minutes, and the alloy solution should be poured.

[0036] The above is a detailed description of the technical solution for reinforcing the mold shell by wrapping carbon fiber cloth, including five process steps: pre-configuration of mold shell slurry, preparation of the mold shell making environment, control of the number of mold shell making layers, addition of carbon fiber cloth after mold shell making, and cleaning and inspection of the mold shell.

[0037] The present invention reinforces the mold shell by wrapping carbon fiber cloth outside the mold shell, utilizes the high strength and heat resistance of the carbon fiber cloth to improve the strength of the mold shell, avoids the mold shell from cracking or deformation during the casting process, and utilizes the good thermal conductivity of the carbon fiber cloth to improve the heat conduction effect of the mold shell, so that the temperature gradient of the casting is more uniform. The carbon fiber cloth has a low thermal expansion coefficient, which can relieve the thermal stress between the casting and the mold shell, avoid deformation or cracking of the casting, and solve the problem of mismatched thermal expansion coefficients. The carbon fiber cloth is wrapped after the mold shell is pre-baked, so that the carbon fiber cloth can be prevented from being heated to high temperature and then cooled in the pre-baking stage, resulting in the failure of the strength. The present invention effectively solves the shortcomings of the existing single crystal directional mold shell technology, improves the strength, thermal conductivity and thermal expansion coefficient matching of the mold shell, thereby improving the quality and forming effect of the casting.

[0038] The heavy-duty gas large-size hollow directional blade shell prepared by this casting shell making process has a low failure rate, good casting surface integrity, and the blade contour size meets the design standard of the drawing. The contour rework rate of the casting shell making process is low, and the overall rework area of ​​the blade is within 10%, which greatly shortens the rework time and greatly reduces the manufacturing cost of the product. A large-scale production process system for heavy-duty gas turbine blades has been established, reaching the international advanced level in terms of product comprehensive performance, geometric dimensions and overall quality, and realizing mass production and application.

[0039] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0040] Obviously, the embodiments described above are only some embodiments of the present invention, rather than all embodiments, but do not limit the patent scope of the present invention. The present invention can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Although the present invention has been described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacements for some of the technical features therein. Any equivalent structure made using the contents of the present invention specification, directly or indirectly used in other related technical fields, is also within the scope of patent protection of the present invention.

Claims

1. A shell manufacturing process for preventing large-size directional shell expansion, characterized in that: The shell is a turbine blade shell of a heavy-duty gas turbine, and its manufacturing process includes the following steps: 1) Pre-configuration of shell slurry: According to the requirements of shell reinforcement, select appropriate shell slurry components, and configure, mix and prepare slurry according to the selected shell slurry components; 2) Preparation of the shell making environment: the shell making temperature is 20-25℃, the humidity is 40-60%, and a robot and an automatic control system are configured; 3) Control of the number of shell layers: There are four types of shells, from inside to outside, namely surface layer, transition layer, reinforcement layer and sealing layer; 4) Shell dewaxing: Use hot air or steam to heat the shell to melt and discharge the wax core. After dewaxing is completed, pre-bake the shell; 5) Shell outer surface treatment: according to the outer surface size of the shell, cut the carbon fiber cloth, wrap it outside the shell after wetting, and dry it naturally for more than 24 hours; 6) Cleaning and inspection of the shell: After the shell is made, use high-pressure air to flush the inner cavity to remove residual impurities, use methylene blue solution to detect leakage, and observe whether there is leakage. Finally, use pure water to flush the inner cavity of the shell to clean up the methylene blue solution and other residues.

2. A shell manufacturing process for preventing large-size directional shell expansion according to claim 1, characterized in that: The medium-sized shell slurry in step 1) comprises zircon powder, silica sol, a wetting agent and a defoaming agent.

3. A shell manufacturing process for preventing large-size directional shell expansion according to claim 1, characterized in that: In the step 3), the material of the surface layer is 100-200 mesh zircon powder, which is used to increase the surface smoothness and hardness of the mold shell. The material of the transition layer is a mixture of 100-200 mesh zircon powder and 70-150 mesh zircon powder of the surface layer, which is used to connect the surface layer and the reinforcement layer. The material of the reinforcement layer is 50-120 mesh zircon powder and mullite particles, which are used to enhance the strength and rigidity of the mold shell. The material of the sealing layer is 100-200 mesh quartz sand, which is used to protect the mold shell and the reinforcement layer.

4. A shell manufacturing process for preventing large-size directional shell expansion according to claim 1, characterized in that: In the step 5), the carbon fiber cloth is immersed in the slurry of the reinforcement layer to wet the carbon fiber cloth, and before the carbon fiber cloth is attached to the shell, the outer surface of the shell is wetted with the slurry of the reinforcement layer to tightly attach the wetted carbon fiber cloth to the shell surface.

5. A shell manufacturing process for preventing large-size directional shell expansion according to claim 1, characterized in that: In the step 5), the carbon fiber cloth is 3K240G twill shaped carbon fiber cloth.

6. A shell manufacturing process for preventing large-size directional shell expansion according to claim 1, characterized in that: In the step 5), the carbon fiber cloth wrapped around the blade body is divided into three sections according to the height, and the connection between the carbon fiber cloth wrapped in the same section is located at the back of the blade, and the tenon of the blade is wrapped with a whole piece of carbon fiber cloth.