Spherical-like silver powder preparation method and spherical-like silver powder
By adding crystal-form control agents and controlling reaction conditions to the preparation of photovoltaic silver powder, the spherical silver powder is formed, which solves the problems of low sintering activity and high cost of existing photovoltaic silver powder, and realizes efficient silver powder preparation, which is suitable for printing solar panels.
Patent Information
- Application Number
- CN202411422278.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing photovoltaic silver powder has low sintering activity and high cost, making it difficult to meet the photovoltaic industry's demand for reduced unit consumption.
By adding crystal form control agent, the synchronous addition rate and pH of the oxide liquid and reducing liquid are controlled to form spherical silver powder, which improves sintering activity and printing properties.
The prepared spherical silver powder has high sintering activity and excellent printing properties. It is suitable for industrial mass production. The particle size and specific surface area are within the preset range and are suitable for printing solar panels.
Smart Images

Figure CN119035533A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of preparation of new precious metal materials, and in particular to a method for preparing quasi-spherical silver powder and the quasi-spherical silver powder. Background Art
[0002] Photovoltaic silver paste has become the main raw material for printed solar panels due to its excellent rheological and conductive properties. Silver powder, as the main conductive phase in solar cell silver paste, accounts for about 90% of the mass ratio in the silver paste, which plays an important role in the electrical properties and cost of the silver paste. With the development demand of the photovoltaic industry to reduce the unit consumption of solar cells, improving the sintering activity of silver powder and reducing the cost of silver powder are the main research directions of photovoltaic silver powder. Summary of the invention
[0003] The purpose of the present application is to provide a method for preparing quasi-spherical silver powder and quasi-spherical silver powder, wherein a quasi-spherical silver powder formed by aggregation of flaky silver powder is generated by adding a crystal control agent, and the spherical silver powder has high sintering activity and excellent printability.
[0004] In a first aspect, an embodiment of the present application provides a method for preparing a spherical powder, comprising:
[0005] preparing an oxidation solution, an initial neutralization solution and a reduction solution respectively;
[0006] adding a crystal form controlling agent to the initial neutralized solution to obtain a neutralized solution;
[0007] The oxidizing solution and the reducing solution are added to the neutralizing solution at a constant rate to obtain a mixed reaction solution;
[0008] After the preset reaction time, the mixed reaction liquid is subjected to precipitation separation to obtain spherical silver powder particles.
[0009] In some possible embodiments, the crystal form control agent is at least one of sodium phosphate, methyl phosphate, ammonium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, and ammonium dihydrogen phosphate.
[0010] In some possible embodiments, silver nitrate is dissolved in the oxidizing solution, a dispersant is dissolved in the initial neutralizing solution, and the added amount of the dispersant is 1-15% of the mass of the silver nitrate.
[0011] In some possible embodiments, the dispersant is one of polyethylene glycol, polyvinyl pyrrolidone, Tween and sodium dodecyl sulfate.
[0012] In some possible embodiments, the added amount of the crystal form control agent is 0-5% of the mass of the silver nitrate.
[0013] In some possible embodiments, after preparing the oxidation solution, the initial neutralization solution and the reduction solution respectively, the method further comprises:
[0014] A pH regulator is added to the oxidizing solution to adjust the pH value of the oxidizing solution to a preset pH range to obtain a new oxidizing solution.
[0015] In some possible embodiments, the step of adding the oxidizing solution and the reducing solution to the neutralizing solution at a constant rate to obtain a mixed reaction solution comprises:
[0016] The new oxidizing solution is added to the neutralizing solution at a first constant addition rate, and the reducing solution is added to the neutralizing solution at a second constant addition rate to obtain a mixed reaction solution.
[0017] In some possible embodiments, the pH adjuster is at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.
[0018] In some possible embodiments, the spherical silver powder has a particle size of 1-1.5 μm and a bulk density of 3-5 g / cm 3 , specific surface area 0.4-0.6㎡ / g.
[0019] In a second aspect, an embodiment of the present application provides a quasi-spherical silver powder, which is prepared by the quasi-spherical silver powder preparation method as described in any one of the above items.
[0020] The present application provides a method for preparing quasi-spherical silver powder and quasi-spherical silver powder, comprising: preparing an oxidizing solution, an initial neutralizing solution and a reducing solution respectively; adding a crystal form control agent to the initial neutralizing solution to obtain a neutralizing solution; adding the oxidizing solution and the reducing solution to the neutralizing solution at a constant rate to obtain a mixed reaction solution; after a preset reaction time, precipitating and separating the mixed reaction solution to obtain silver powder particles. The method for preparing the quasi-spherical silver powder provided by the present application is simple, has low preparation requirements and is conducive to industrial mass production; and the prepared silver powder is formed by aggregation of flaky microcrystals, has a high sphericity, a large specific surface area, and a high sintering activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.
[0022] Figure 1 It is a schematic diagram of the process of preparing spherical silver powder provided in the embodiment of the present application;
[0023] Figure 2 This is a scanning electron microscope image of the silver powder prepared in Example 1 using the method of the present application;
[0024] Figure 3 This is a scanning electron microscope image of silver powder prepared by Example 2 of the method of the present application;
[0025] Figure 4 This is a scanning electron microscope image of silver powder prepared by Example 3 of the method of the present application;
[0026] Figure 5 This is a scanning electron microscope image of the silver powder prepared in Comparative Example 1 using the method of the present application;
[0027] Figure 6 This is a scanning electron microscope image of the silver powder prepared in Comparative Example 2 using the method of the present application. DETAILED DESCRIPTION
[0028] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.
[0029] In the following description of the present application, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.
[0030] In the following description of the present application, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged with a specific order or sequence where permitted, so that the embodiments of the present application described here can be implemented in an order other than that illustrated or described here.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.
[0032] The following is a detailed description with reference to specific embodiments. It should be noted that the serial numbers of the following embodiments are not intended to limit the preferred order of the embodiments. The present application improves the specific steps of the method for preparing spherical silver powder, which is described in detail below.
[0033] See also Figure 1 , Figure 1 The schematic diagram of the process of preparing quasi-spherical silver powder provided in the embodiment of the present application is a schematic diagram of the process of preparing quasi-spherical silver powder. The method of preparing quasi-spherical silver powder may specifically include the following steps:
[0034] 101. Prepare oxidizing solution, initial neutralizing solution and reducing solution respectively.
[0035] The method for preparing spherical silver powder provided in the present application still mainly converts silver ions into silver powder particles through redox reaction, so it is necessary to separately prepare an oxidizing solution including silver ions and a reducing solution for reducing the silver ions in the oxidizing solution; it is also necessary to prepare an initial neutralizing solution, which mainly provides a reaction environment, and the oxidizing solution and the reducing solution are added to the neutralizing solution respectively, so that the oxidizing solution and the reducing solution undergo redox reaction in the neutralizing solution. At the same time, the neutralizing solution is usually prepared with a dispersant, and the dissolved dispersant can effectively control the dispersion of silver ions and reducing ions, and better improve the efficiency of the redox reaction. At the same time, the dispersant in the present application will also affect the shape of the silver powder.
[0036] In some embodiments, the silver nitrate solid can be configured as a silver nitrate solution to obtain an oxidizing solution, and the reducing agent can be configured as a reducing solution; and the mass concentration of silver nitrate in the oxidizing solution is 10-25%; the mass concentration of the reducing agent in the reducing solution is 10-20%. The amount of dispersant added to the initial neutralizing solution can be 1-15% of the mass of silver nitrate. In some embodiments, the reducing agent can be at least one of glucose, sodium borohydride, formaldehyde, ascorbic acid, hydrazine hydrate, hydroquinone, alkanolamine or hydrogen peroxide; the dispersant can be one of polyethylene glycol, polyvinyl pyrrolidone, Tween and sodium dodecyl sulfate, wherein Tween can be Tween 40. In the embodiments of the present application, the specific methods and steps for preparing the oxidizing solution, reducing solution and initial neutralizing solution can refer to the prior art and are not limited here. In the embodiments of the present application, the solution temperature of the prepared oxidizing solution, reducing solution and initial neutralizing solution can be controlled within the range of 10-25°C.
[0037] 102. Add a crystal form control agent to the initial neutralized solution to obtain a neutralized solution.
[0038] 103. The oxidizing solution and the reducing solution are added to the neutralizing solution simultaneously at a constant rate to obtain a mixed reaction solution.
[0039] After the oxidizing solution and the reducing solution are prepared separately, the two need to be mixed to carry out an oxidation-reduction reaction; and in the embodiment of the present application, before the oxidizing solution and the reducing solution are added to the initial neutralizing solution, a crystal form controller needs to be added to the initial neutralizing solution to obtain a neutralizing solution. Among them, the crystal form controller can control the shape and growth process of the silver powder, and finally obtain spherical silver powder particles. In the embodiment of the present application, the crystal form controller can be at least one of sodium phosphate, methyl phosphate, ammonium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, and ammonium dihydrogen phosphate. After the crystal form controller is first added to the initial neutralizing solution and fully mixed to obtain a neutralizing solution, the neutralizing solution containing the crystal form controller is used for an oxidation-reduction reaction. The amount of the crystal form controller added can be 0-5% of the mass of silver nitrate.
[0040] In the above embodiments, after the oxidizing solution is prepared, the oxidizing solution cannot be used directly, and a pH adjusting agent needs to be added to the oxidizing solution to adjust the pH value of the oxidizing solution to a preset pH range to obtain a new oxidizing solution. In some embodiments, the pH value of the oxidizing solution can be adjusted to 1-3 to obtain a new oxidizing solution. Then, the new oxidizing solution after pH adjustment is added to the neutralizing solution at a first constant addition rate, and the reducing solution is added to the neutralizing solution at a second constant addition rate to obtain a mixed reaction solution. At this time, the components in the mixed reaction solution will undergo an oxidation-reduction reaction under a certain pH environment to obtain silver powder. In some embodiments, the pH adjusting agent is at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.
[0041] In the above embodiment, when the redox reaction is actually carried out, the reducing solution and the new oxidizing solution after adjusting the pH are added to the neutralizing solution containing the crystal form control agent respectively to obtain a mixed reaction solution. In some embodiments, the new oxidizing solution can be added to the neutralizing solution at a first constant addition rate, and the reducing solution can be added to the neutralizing solution at a second constant addition rate to obtain a mixed reaction solution. That is, when the oxidizing solution and the reducing solution are actually added, it is not only necessary to add them at the same time, but also necessary to control the addition rate of both to control the process of the redox reaction, and then control the shape and size of the silver powder particles finally generated. At the same time, in the embodiment of the present application, it is usually necessary to completely add the new oxidizing solution and the reducing solution to the neutralizing solution within a certain period of time. Among them, the addition time of the new oxidizing solution and the reducing solution can be 3-5 minutes, that is, both are completely added to the neutralizing solution within a period of 3-5 minutes; and the size of the first constant addition rate corresponding to the oxidizing solution and the second addition rate corresponding to the reducing solution can be determined according to the amount of the oxidizing solution and the reducing solution actually added, which is not limited in this application.
[0042] 104. After the preset reaction time, the mixed reaction liquid is precipitated and separated to obtain silver powder particles.
[0043] After the redox reaction of a preset time, the obtained silver powder particles are suspended in the mixed reaction liquid, and the silver powder particles in the mixed reaction liquid need to be separated to obtain the final quasi-spherical silver powder. Specifically, after five minutes of reaction, the mixed reaction liquid can be allowed to settle to obtain a layered upper liquid and lower sediment; the sediment is separated and further processed. Among them, the sediment is the silver powder particles obtained by the redox reaction, but there are impurities attached to the sediment, so the sediment needs to be further cleaned to obtain pure silver powder particles without impurities. In other embodiments, the mixed reaction liquid can also be washed first, and the sediment is separated after being cleaned. Finally, the particles are dried at a certain temperature for a certain period of time to obtain the final quasi-spherical silver powder. In a specific embodiment, the quasi-spherical silver powder particles can be obtained by drying at 40-100°C or more specifically 50-80°C for 2-6 hours.
[0044] The method for preparing quasi-spherical silver powder provided in the embodiment of the present application comprises: preparing an oxidizing solution, an initial neutralizing solution and a reducing solution respectively; adding a crystal form control agent to the initial neutralizing solution to obtain a neutralizing solution; adding the oxidizing solution and the reducing solution to the neutralizing solution at a constant rate to obtain a mixed reaction solution; after a preset reaction time, precipitating and separating the mixed reaction solution to obtain silver powder particles. The method for preparing quasi-spherical silver powder provided in the present application is simple, has low preparation requirements and is conducive to industrial mass production; and the prepared silver powder is formed by aggregation of flaky microcrystals, has a high sphericity, a large specific surface area, and a high sintering activity.
[0045] It should be noted that the method for preparing quasi-spherical silver powder provided in the embodiment of the present application is to first prepare flaky or strip-shaped silver powder, and then aggregate the flaky or strip-shaped silver powder to form quasi-spherical silver powder. The quasi-spherical silver powder prepared in this way has the advantages of regular morphology and high activity of flaky silver powder, and also has the excellent printability of spherical silver powder, and can be used in mainstream TOPCON batteries. The preparation process of the method for preparing quasi-spherical silver powder provided in the present application is described in detail below in conjunction with specific embodiments.
[0046] Embodiment 1:
[0047] 1.6 kg of silver nitrate solid was weighed to prepare a silver nitrate solution with a mass fraction of 15%, i.e., an oxidizing solution, and nitric acid was added thereto to adjust the pH to 2.2, thereby obtaining a new silver nitrate solution or a new oxidizing solution after pH adjustment; 0.86 kg of ascorbic acid was weighed as a reducing agent to prepare a reducing agent solution with a mass concentration of 10%. 0.1 kg of polyvinyl pyrrolidone was weighed as a dispersant to prepare an initial neutralizing agent solution with a mass concentration of 5%, and 15 g of dihydrogen phosphate was added thereto as a crystal form control agent to obtain a final neutralizing agent solution.
[0048] The temperature of the reaction liquid was maintained at 20° C. and the stirring speed was 400 rpm. New oxidizing liquid and reducing liquid were simultaneously added dropwise to the neutralizing liquid at a first constant rate and a second constant rate, and the addition time was controlled to be 5 minutes.
[0049] After the addition was completed, the reaction was continued for 5 minutes, and the mixed reaction liquid was washed with deionized water and ethanol, and the upper clear liquid was filtered to obtain the lower sediment after standing for a period of time. The sediment was dried at 60°C for 30 minutes and filtered through a 500-mesh sieve to obtain the final spherical silver powder. The actual particle size D50 of the obtained silver powder was 1.2μm, the specific surface area was 0.55㎡ / g, and the scanning electron microscope image was shown in Figure 2 .
[0050] Embodiment 2:
[0051] 1.6 kg of silver nitrate solid was weighed to prepare a silver nitrate solution with a mass fraction of 15%, i.e., an oxidizing solution, and nitric acid was added thereto to adjust the pH to 2.2, thereby obtaining a new silver nitrate solution or a new oxidizing solution after pH adjustment; 0.86 kg of ascorbic acid was weighed as a reducing agent to prepare a reducing agent solution with a mass concentration of 10%. 0.1 kg of polyvinyl pyrrolidone was weighed as a dispersant to prepare an initial neutralizing agent solution with a mass concentration of 5%, and 50 g of dihydrogen phosphate was added thereto as a crystal form control agent to obtain a final neutralizing agent solution.
[0052] The temperature of the reaction liquid was maintained at 20° C. and the stirring speed was 400 rpm. New oxidizing liquid and reducing liquid were simultaneously added dropwise to the neutralizing liquid at a first constant rate and a second constant rate, and the addition time was controlled to be 5 minutes.
[0053] After the addition was completed, the reaction was continued for 5 minutes, and the mixed reaction liquid was washed with deionized water and ethanol, and the upper clear liquid was filtered to obtain the lower sediment after standing for a period of time. The sediment was dried at 60°C for 30 minutes and filtered through a 500-mesh sieve to obtain the final spherical silver powder. The actual particle size D50 of the obtained silver powder was 1.1 μm, the specific surface area was 0.50 m2 / g, and the scanning electron microscope image was shown in FIG. Figure 3 .
[0054] The difference between Example 2 and Example 1 is that the amount of the crystal form control agent is controlled. By controlling the amount of the crystal form control agent, spherical silver powders with different particle sizes and specific surface areas can be generated; and the structure of the spherical silver powder does not change significantly.
[0055] Embodiment 3:
[0056] 1.6 kg of silver nitrate solid was weighed to prepare a silver nitrate solution with a mass fraction of 15%, i.e., an oxidizing solution, and nitric acid was added thereto to adjust the pH to 2.2, thereby obtaining a new silver nitrate solution or a new oxidizing solution after pH adjustment; 0.86 kg of ascorbic acid was weighed as a reducing agent to prepare a reducing agent solution with a mass concentration of 10%. 0.1 kg of polyvinyl pyrrolidone was weighed as a dispersant to prepare an initial neutralizing agent solution with a mass concentration of 5%, and 15 g of dihydrogen phosphate was added thereto as a crystal form control agent to obtain a final neutralizing agent solution.
[0057] The solution temperature of the oxidizing solution and the reducing solution was controlled at 30° C. and the stirring speed was 400 rpm. The new oxidizing solution and the reducing solution were simultaneously added dropwise to the neutralizing solution at a first constant rate and a second constant rate, and the adding time was controlled at 5 minutes.
[0058] After the addition was completed, the reaction was continued for 5 minutes, and the mixed reaction liquid was washed with deionized water and ethanol, and the upper clear liquid was filtered to obtain the lower sediment after standing for a period of time. The sediment was dried at 60°C for 30 minutes and filtered through a 500-mesh sieve to obtain the final spherical silver powder. The actual particle size D50 of the obtained silver powder was 1.1 μm, the specific surface area was 0.35 m2 / g, and the scanning electron microscope image was shown in Figure 4 .
[0059] The difference between Example 3 and Example 1 is that the reaction liquid temperature of the mixed solution during the redox reaction is different; although the structure of the spherical silver powder has not changed significantly, the difference in temperature affects the particle size and specific surface area of the spherical silver powder finally obtained, so it is also necessary to control the solution temperature of the oxidizing solution and the reducing solution within a reasonable range.
[0060] Comparative Example 1:
[0061] 1.6 kg of silver nitrate solid was weighed to prepare a silver nitrate solution with a mass fraction of 15%, i.e., an oxidizing solution, and nitric acid was added thereto to adjust the pH to 2.2, thereby obtaining a new silver nitrate solution or a new oxidizing solution after pH adjustment; 0.86 kg of ascorbic acid was weighed as a reducing agent to prepare a reducing agent solution with a mass concentration of 10%. 0.1 kg of polyvinyl pyrrolidone was weighed as a dispersant to prepare an initial neutralizing agent solution with a mass concentration of 5%.
[0062] The temperature of the reaction liquid was maintained at 20° C. and the stirring speed was 400 rpm. The new oxidizing liquid and the reducing liquid were simultaneously added dropwise to the initial neutralizing liquid at a first constant rate and a second constant rate, and the addition time was controlled to be 5 minutes.
[0063] After the addition was completed, the reaction was continued for 5 minutes, and the mixed reaction liquid was washed with deionized water and ethanol, and the upper clear liquid was filtered to obtain the lower sediment after standing for a period of time. The sediment was dried at 60°C for 30 minutes and filtered through a 500-mesh sieve to obtain the final spherical silver powder. The actual particle size D50 of the obtained silver powder was 1.1 μm, the specific surface area was 0.4 m2 / g, and the scanning electron microscope image was shown in FIG. Figure 5 .
[0064] The difference between Comparative Example 1 and Example 1 is that no crystal form control agent is added. Although the particle size and specific surface area of the silver powder prepared in Comparative Example 1 are within the preset range, according to Figure 5 It can be determined that a large number of spike structures are formed on the silver powder prepared in Comparative Example 1, which is completely different from the structure of the silver powder prepared in Example 1. Therefore, it is impossible to form such a structure without adding a crystal form control agent. Figure 2 The spherical silver powder shown.
[0065] Comparative Example 2:
[0066] 1.6 kg of silver nitrate solid was weighed to prepare a silver nitrate solution with a mass fraction of 15%, i.e., an oxidizing solution, and nitric acid was added thereto to adjust the pH to 2.2, thereby obtaining a new silver nitrate solution or a new oxidizing solution after pH adjustment; 0.86 kg of ascorbic acid was weighed as a reducing agent to prepare a reducing agent solution with a mass concentration of 10%. 0.1 kg of polyethylene glycol was weighed as a dispersant to prepare an initial neutralizing agent solution with a mass concentration of 5%, and 15 g of dihydrogen phosphate was added thereto as a crystal form control agent to obtain a final neutralizing agent solution.
[0067] The temperature of the reaction liquid was maintained at 20° C. and the stirring speed was 400 rpm. New oxidizing liquid and reducing liquid were simultaneously added dropwise to the neutralizing liquid at a first constant rate and a second constant rate, and the addition time was controlled to be 5 minutes.
[0068] After the addition was completed, the reaction was continued for 5 minutes, and the mixed reaction liquid was washed with deionized water and ethanol, and the upper clear liquid was filtered to obtain the lower sediment after standing for a period of time. The sediment was dried at 60°C for 30 minutes and filtered through a 500-mesh sieve to obtain the final spherical silver powder. The actual particle size D50 of the obtained silver powder was 1.2μm, the specific surface area was 0.55㎡ / g, and the scanning electron microscope image was shown in Figure 6 .
[0069] The difference between Comparative Example 2 and Example 1 is that the dispersant is polyethylene glycol, that is, the neutralizing solution is different, and the particle size of the spherical silver powder finally obtained exceeds the preset silver powder particle size range, and according to Figure 6It can be determined that the aggregation degree of the silver powder prepared in Comparative Example 2 is not as concentrated as that of the silver powder in Example 1, and the structure of the silver powder has actually changed to a certain extent. Therefore, it can be determined that different dispersants will also affect the structure and particle size of the silver powder, and the material selection of the crystal form control agent and the material selection of the dispersant need to be controlled in this application.
[0070] The present application also provides a quasi-spherical silver powder, which is prepared by using the quasi-spherical silver powder preparation method provided by any of the above embodiments, and thus has all the same beneficial effects, and this embodiment will not be described in detail herein.
[0071] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0072] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing spherical silver powder, characterized in that: include: preparing an oxidation solution, an initial neutralization solution and a reduction solution respectively; Adding a crystal form control agent to the initial neutralized solution to obtain a neutralized solution; The oxidizing solution and the reducing solution are added to the neutralizing solution at a constant rate to obtain a mixed reaction solution; After the preset reaction time, the mixed reaction liquid is subjected to precipitation separation to obtain spherical silver powder particles.
2. The method for preparing spherical silver powder according to claim 1, characterized in that: The crystal form control agent is at least one of sodium phosphate, methyl phosphate, ammonium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, and ammonium dihydrogen phosphate.
3. The method for preparing spherical silver powder according to claim 1, characterized in that: Silver nitrate is dissolved in the oxidizing solution, and a dispersant is dissolved in the initial neutralizing solution. The added amount of the dispersant is 1-15% of the mass of the silver nitrate.
4. The method for preparing spherical silver powder according to claim 3, characterized in that: The dispersant is one of polyethylene glycol, polyvinyl pyrrolidone, Tween and sodium dodecyl sulfate.
5. The method for preparing spherical silver powder according to claim 3, characterized in that: The added amount of the crystal form control agent is 0-5% of the mass of the silver nitrate.
6. The method for preparing spherical silver powder according to claim 1, characterized in that: After preparing the oxidation solution, the initial neutralization solution and the reduction solution respectively, the method further comprises: A pH regulator is added to the oxidizing solution to adjust the pH value of the oxidizing solution to a preset pH range to obtain a new oxidizing solution.
7. The method for preparing spherical silver powder according to claim 6, characterized in that: The step of adding the oxidizing solution and the reducing solution to the neutralizing solution at a constant rate to obtain a mixed reaction solution comprises: The new oxidizing solution is added to the neutralizing solution at a first constant adding rate, and the reducing solution is added to the neutralizing solution at a second constant adding rate to obtain a mixed reaction solution.
8. The method for preparing spherical silver powder according to claim 6, characterized in that: The pH regulator is at least one of methylamine, trimethylamine, triethylamine, ammonia water, ammonium carbonate, sodium carbonate, sodium hydroxide or potassium hydroxide.
9. The method for preparing spherical silver powder according to claim 1, characterized in that: The quasi-spherical silver powder has a particle size of 1-1.5 μm and a bulk density of 3-5 g / cm 3 , specific surface area 0.4-0.6㎡ / g.
10. A quasi-spherical silver powder, characterized in that: The spherical silver powder is prepared by the method for preparing the spherical silver powder according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method and application of high-purity spherical silver powder
CN119772192A
Blocky stacked spherical copper powder and preparation method thereof
CN120421526A
Nanometer aggregated silver powder and preparation method thereof
CN122322461A