Composite material photovoltaic frame and preparation method and preparation device thereof

Through the low-temperature and high-temperature batch impregnation process of continuous fiber-reinforced thermoplastic composites, the problems of high cost, poor reliability and difficult recycling of photovoltaic frame materials are solved, and efficient and low-cost photovoltaic frame preparation is achieved, which improves mechanical performance and pultrusion speed .

CN119036896AActive Publication Date: 2024-11-29LONGI GREEN ENERGY TECH CO LTD

Patent Information

Application Number
CN202410993065.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-29
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing photovoltaic frame materials have high cost, high carbon tax, limited production capacity, insufficient reliability in corrosion scenarios, and difficult recycling of thermosetting materials, unsatisfactory impregnation effect of thermoplastic resins, slow pultrusion speed, and high process cost.

Method used

The continuous fiber-reinforced thermoplastic composite material is adopted, and the fiber impregnation and polymerization is used to use a monomer solution to improve the bonding degree between fiber and resin, reduce porosity, and improve the mechanical properties and pultrusion speed of the frame.

Benefits of technology

The photovoltaic frame with low cost, easy recycling, easy repair and excellent mechanical properties is achieved, solving the problems of difficult recycling of thermoset materials and poor impregnation effect of thermoplastic materials, and reducing processing temperature and process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure HDA0004959471410000011
    Figure HDA0004959471410000011
Patent Text Reader

Abstract

The invention relates to a preparation method of a thermoplastic composite material photovoltaic frame, which comprises the following steps: arranging and shaping continuous fibers, introducing a fibrofelt into the surface of an inner cavity of the shape to cover the continuous fibers to form a fiber preform, and introducing the fiber preform into a mold; injecting a mixture comprising a chemical monomer, a reaction aid and a filler into the mold at a low temperature to perform primary impregnation on the fiber preform, and introducing fiber cloth at a high temperature to cover the surface of the fiber preform subjected to primary impregnation so as to form a composite preform, injecting a mixture comprising a chemical monomer, a reaction aid and a filler into the mold to perform secondary impregnation on the fiber cloth of the composite preform, and polymerizing the chemical monomer in the composite preform subjected to twice impregnation at a polymerization temperature to obtain the fiber cloth of the composite preform. And cooling the polymerized fiber preform to obtain a frame profile, and processing the frame profile into the photovoltaic frame.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the photovoltaic field, and in particular to a thermoplastic bio-based composite photovoltaic frame and a preparation method and a preparation device thereof. Background Art

[0002] Photovoltaic frames are important structural parts of photovoltaic modules, ensuring the normal operation of power generation functions. They are also the auxiliary materials with the highest cost in photovoltaic modules. Currently, photovoltaic frames are mainly made of aluminum alloy materials, so they face application disadvantages such as high cost, high carbon tax, and limited production capacity. Moreover, in heavy corrosion scenarios (such as oceans, chemical plants, farms, etc.), the reliability of photovoltaic frames made of existing aluminum alloy materials is insufficient.

[0003] At present, some researchers have considered using continuous fiber reinforced composite materials. This is because continuous fiber reinforced composite materials have the advantages of high strength, low cost, low carbon tax, corrosion resistance, etc., especially continuous glass fiber reinforced polyurethane-based composite materials have been valued by the photovoltaic industry and have begun mass production and pilot applications. However, as a thermosetting material, polyurethane-based composite materials face the dilemma of difficult recycling. In contrast, continuous fiber reinforced thermoplastic composite materials have the advantages of recyclability, high toughness, and easy repair on the basis of thermosetting, and are currently recognized as the best photovoltaic frame alternative material in this field. Summary of the invention

[0004] Continuous fiber reinforced thermoplastic composite frames are generally manufactured using a melt infusion pultrusion process. After the molten thermoplastic resin is impregnated with the continuous fiber, it is passed through a molding die and cooled to obtain a profile. However, the viscosity of the thermoplastic resin melt is generally high, the impregnation effect is not ideal, internal defects are easily generated, and the pultrusion speed is slow. Therefore, the pultrusion process still needs to be improved.

[0005] At present, continuous fiber reinforced thermosetting composite frames represented by polyurethane have the problem of difficult recycling; however, the manufacturing of thermoplastic composite frames has the problems of difficult resin impregnation, slow pultrusion speed and high process cost.

[0006] The present application aims to solve the problems existing in the above-mentioned prior art and attempts to improve the existing impregnation and pultrusion processes. The present application uses thermoplastic resin monomers for fiber impregnation and develops a continuous preparation process, thereby realizing the efficient preparation of photovoltaic frames using thermoplastic composite materials.

[0007] This application involves the following solutions:

[0008] The present application provides a method for preparing a thermoplastic composite photovoltaic frame, which includes the following steps: using continuous fibers and fiber felts to form a fiber preform; introducing the fiber preform into a mold; injecting a monomer solution into the mold at a low temperature to impregnate the fiber preform once, introducing a fiber cloth to cover the surface of the fiber preform that has been impregnated once to form a composite preform at a high temperature, injecting the monomer solution into the mold to impregnate the fiber cloth of the composite preform twice, polymerizing the monomers in the composite preform that has been impregnated twice at a polymerization temperature, cooling the polymerized fiber preform, and processing it to obtain a photovoltaic frame.

[0009] The present application performs two batch impregnations and one-piece reaction pultrusion molding on a preform composed of continuous fibers, fiber mats, and fiber cloth, thereby improving the mechanical properties and pultrusion speed of the thermoplastic composite frame. The present application also solves the problems in the prior art that the lateral strength and stiffness are poor, the cost is high, and the conventional impregnation cannot fully impregnate the mesh cloth. The composite photovoltaic frame prepared by the method of the present application is low-cost, easy to recycle, has high toughness, and is easy to repair.

[0010] In some embodiments, the low temperature ranges from 80° C. to 170° C., or the high temperature ranges from 120° C. to 180° C., or the polymerization temperature ranges from 140° C. to 245° C. In this temperature range, the internal unidirectional fiber can be better impregnated under low temperature conditions, and the secondary impregnation and curing of the thermoplastic resin can be performed under high temperature conditions.

[0011] In some embodiments, before being introduced into the frame forming mold, the fiber preform is further preheated, preferably at a temperature ranging from 90° C. to 180° C. The preheating step can be more conducive to the effective implementation of the two polymerizations of the present application.

[0012] In some embodiments, the mold includes a low temperature zone and a high temperature zone in sequence in the direction of fiber cloth transportation, and the primary impregnation and secondary impregnation are performed in the low temperature zone and the high temperature zone, respectively. The low temperature zone mainly serves to provide a relatively low temperature so as to better impregnate the internal unidirectional fibers, and the high temperature zone mainly serves to provide a relatively high temperature so as to better achieve secondary impregnation and curing of the thermoplastic resin. Using monomers for two batch impregnations can fully composite with the fiber preform, reduce porosity, improve frame performance, improve the strength of the composite frame in the direction perpendicular to the fibers, and enhance the fiber woven cloth and fiber felt constituting the outer surface of the frame and the inner cavity surface. This overcomes the defect that a single impregnation of thermoplastic resin is difficult to fully penetrate the fiber preform.

[0013] In some embodiments, the volume ratio of the mixture used in the first dipping and the mixture used in the second dipping is in the range of (70-90): (30-10). In the two dipping processes, by further optimizing the ratio of the monomer solution injected by the two dippings, the balance between the strength in the length direction of the frame and the strength in the direction perpendicular to the length direction can be better coordinated to achieve more excellent frame performance. The applicant has made a lot of optimizations to this and found that the volume ratio of the mixture used in the first dipping and the mixture used in the second dipping is maintained within a certain range, which can significantly improve the performance of the final product, for example, the mechanical properties are excellent as a whole, the strength in the length direction of the frame is excellent, and the strength in the direction perpendicular to the length direction is also good. If not controlled, it may result in poor strength in the length direction of the frame, or poor strength in the direction perpendicular to the length direction, which will cause the overall performance of the frame to deteriorate.

[0014] In some embodiments, the step of forming a fiber preform using continuous fibers and fiber mats includes: arranging the continuous fibers into a shape, introducing fiber mats into the inner cavity surface of the shape to cover the continuous fibers to form a fiber preform. The fiber preform formed in this way can better form a frame, and finally obtain a frame profile with high mechanical strength.

[0015] In some embodiments, cooling and processing the fiber preform to obtain a photovoltaic frame includes the following steps: cooling the fiber preform that has completed the polymerization reaction to obtain a frame profile; cutting the frame profile to obtain a fixed-length profile, and online grinding and painting the fixed-length profile to obtain a photovoltaic frame.

[0016] In some embodiments, the monomer solution includes: chemical monomers, reaction aids and fillers; injecting the monomer solution includes the following steps: mixing chemical monomers, reaction aids and fillers from different material tanks through a high-pressure injection head, and injecting the mixture into the mold after uniformly dispersing the mixture through ultrasonic dispersion. In the method of the present application, the use of ultrasonic dispersion treatment can make the mixing and dispersion of the various parts forming the monomer solution more uniform.

[0017] In some embodiments, the chemical monomer is selected from one or more of caprolactam, butyrolactam, valerolactam, undecanoic acid, laurolactam or tridecanolactam; or the reaction aid is selected from one or more of initiator, catalyst, release agent; or the filler is selected from one or more of hollow glass microspheres, calcium carbonate, talc, montmorillonite, titanium dioxide or wollastonite. The selection of the above materials can better achieve the purpose of this application. The chemical monomer used in this application can be fully polymerized, and no extra components will be produced, and no additional post-processing steps are required.

[0018] In some embodiments, when the chemical monomer is caprolactam, butyrolactam or valerolactam, the low temperature ranges from 80°C to 100°C, the high temperature ranges from 120°C to 140°C, the polymerization temperature ranges from 140°C to 160°C, and the preheating temperature is 90°C to 100°C; when the chemical monomer is undecanoic acid, lauryl lactam or tridecanoic acid, the low temperature ranges from 160°C to 170°C, the high temperature ranges from 170°C to 180°C, the polymerization temperature ranges from 180°C to 245°C, and the preheating temperature is 170°C to 180°C. The inventors of the present application select different temperatures for different materials, which is more conducive to uniform impregnation and uniform curing.

[0019] In some embodiments, the continuous fiber is selected from one or more of glass fiber roving, polymer fiber or biomass fiber, preferably the polymer fiber is selected from ultra-high molecular weight polyethylene, polyethylene terephthalate, poly(p-phenylene phthalamide), preferably the biomass fiber is selected from bamboo pulp fiber, hemp pulp fiber and chitosan fiber; the fiber mat is selected from carbon fiber mat, glass fiber mat or polyester fiber mat; or the fiber cloth is selected from glass fiber plain weave cloth, glass fiber twill weave cloth and glass fiber satin weave cloth. The glass fiber plain weave cloth used in this application can better form a frame and has higher mechanical strength.

[0020] The present application provides a preparation device for a thermoplastic composite photovoltaic frame, which includes: a fiber preform forming mechanism, which uses continuous fibers and fiber mats to form a fiber preform; a frame forming mold, which is used to place the fiber preform and can control the temperature and is used to perform impregnation and polymerization reactions of the fiber preform; a glue injection mechanism, which can inject a monomer solution into the mold; a conveying mechanism and a cutting mechanism, which are used to convey the cooled frame to form and process it into a photovoltaic frame; wherein the mold is divided into a low temperature zone and a high temperature zone, and the glue injection mechanism includes a primary impregnation injection channel and a secondary impregnation injection channel, the low temperature zone is connected to the primary impregnation injection channel for the primary impregnation, and the high temperature zone is connected to the secondary impregnation injection channel for the secondary impregnation. Through the above device, two batch impregnations of the chemical monomer mixture can be achieved, which can be fully compounded with the fiber preform, reduce the porosity, and improve the frame performance.

[0021] In some embodiments, in the low temperature zone of the mold, the monomer solution is injected into the mold through the primary impregnation injection channel and the first injection port to perform a primary impregnation on the fiber preform, in the high temperature zone of the mold, a fiber cloth is introduced into the mold to cover the surface of the fiber preform impregnated once to form a composite preform, and the monomer solution is injected into the mold through the secondary impregnation injection channel and the second injection port to perform a secondary impregnation on the fiber cloth of the composite preform, in the high temperature zone of the mold, the monomer in the composite preform impregnated twice is polymerized in the injection mechanism mold; wherein the primary impregnation injection channel and the secondary impregnation injection channel are independent of each other. The low temperature zone mainly performs the impregnation of the internal unidirectional fibers, and the high temperature zone performs the impregnation and curing of the secondary resin. Through the coordination of the low temperature zone and the high temperature zone, it is possible to better coordinate the balance between the strength in the length direction of the frame and the strength in the direction perpendicular to the length direction, and achieve a more excellent frame performance.

[0022] In some embodiments, the preparation device of the present application further includes a temperature control system, which can control the temperature of the mold based on the different monomers used for impregnation and polymerization reactions, and can independently control the mold within the following temperature ranges: the temperature range of the low temperature is 80°C to 170°C, or the temperature range of the high temperature is 120°C to 180°C, or the polymerization temperature range is 140°C to 245°C. By controlling the temperature of the two batch impregnations, the monomer solution can be fully impregnated under different conditions, and further at an appropriate polymerization temperature, the polymerization reaction can be more fully achieved. By precisely controlling the above temperature, the monomer can be fully compounded and polymerized with the fiber preform, and a thermoplastic resin is formed on the surface of the fiber preform, thereby reducing the porosity and improving the frame performance.

[0023] In some embodiments, the preparation device of the present application further comprises: a preheating mechanism, which is used to preheat the fiber preform before being introduced into the frame forming mold, and preferably the temperature control system controls the preheating temperature of the preheating mechanism to be 90° C. to 180° C. The preheating treatment of the preheating mechanism can better achieve impregnation.

[0024] In some embodiments, the injection mechanism controls the volume ratio of the mixture entering the primary dipping injection channel and the mixture entering the secondary dipping injection channel to be in the range of (70-90):(30-10).

[0025] In some embodiments, a temperature control system is provided that controls the temperature of the mold and the preheating mechanism based on the monomers used for impregnation and polymerization.

[0026] When the chemical monomer is caprolactam, butyrolactam or valerolactam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 80°C to 100°C, the temperature control system controls the temperature range of the high temperature zone to be 120°C to 140°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 140°C to 160°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 90°C to 100°C; when the chemical monomer is undecanoic acid tam, lauryl lactam or tridecanoic acid tam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 160°C to 170°C, the temperature control system controls the temperature range of the high temperature zone to be 170°C to 180°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 80°C to 245°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 170°C to 180°C. Through such a setting, the internal unidirectional fiber can be better impregnated under low temperature conditions, secondary impregnation can be performed under high temperature conditions, and the thermoplastic resin can be fully cured at the polymerization temperature.

[0027] The present application provides a thermoplastic composite photovoltaic frame, which comprises the following structures stacked in sequence: a fiber molding having a thermoplastic resin formed on the surface, including continuous fibers and fiber mats; a fiber cloth having a thermoplastic resin formed on the surface; and a weather-resistant coating coated on the fiber cloth. The thermoplastic composite photovoltaic frame has good mechanical properties and pultrusion speed.

[0028] In some embodiments, the thermoplastic resin is obtained by polymerizing a monomer solution including a chemical monomer, a reaction aid and a filler on a fiber molding.

[0029] In some embodiments, the thermoplastic composite photovoltaic frame is prepared by the method described above in the present application or by the preparation device described above in the present application.

[0030] Effects of the Invention

[0031] The preparation method of the thermoplastic composite photovoltaic frame of the present application has the advantages of low monomer viscosity, good impregnation effect and low processing temperature. And the preform composed of continuous fibers, fiber felt and fiber cloth is subjected to two batch impregnations and integrated reaction pultrusion molding, which improves the mechanical properties and pultrusion speed of the thermoplastic composite frame. The existing composite frame surface only has chopped fiber felt, and the lateral strength and rigidity are relatively poor, but if it is replaced with a continuous fiber mesh cloth, its performance may be improved. However, due to the high density of the mesh cloth, if conventional impregnation is used, it cannot effectively improve the strength to prepare a usable frame profile. The method or device of the present application can effectively solve the above problems. The composite photovoltaic frame prepared by the method or device of the present application is low in cost, easy to recycle, high in toughness, and easy to repair.

[0032] In the prior art, thermoplastic resin is usually melted at high temperature and impregnated into fibers, and then pultruded to form a composite material frame. However, in the present application, thermoplastic resin monomer is mixed with additives and fillers, and then ultrasonically dispersed, and in situ polymerized into thermoplastic resin during the process of impregnating fibers, and then pultruded to form a composite material frame. Since thermoplastic resin has a high melting point and a high melt viscosity, the melt viscosity of conventional polyamide is about 10 3 ~10 4 Pa·s, resulting in high processing temperature, so conventional resin impregnation is difficult, composite materials are prone to defects, and pultrusion speed is slow. However, the monomer of the thermoplastic resin used in this application has a low melting point and low viscosity. The conventional monomer lactam melt viscosity is about 10 -2 ~10 -1 Pa·s, so the processing temperature is low, impregnation is easy, the composite material has few defects and the processing speed is fast.

[0033] In the prior art, only a single impregnation is performed using a monomer solution that forms a thermoplastic resin, but the present application uses a monomer solution that forms a thermoplastic resin for two impregnations, and uses the two impregnations to impregnate the fiber preform formed by continuous fibers and fiber mats respectively, and after the first impregnation, the composite preform introduced with the fiber cloth is impregnated for the second time. This impregnation method can greatly improve the strength of the composite material frame in the vertical fiber direction, and the fiber woven cloth and fiber mat that form the outer surface and inner cavity surface of the frame are strengthened. Usually, it is difficult for a thermoplastic resin to fully penetrate the fiber preform by a single impregnation. Using a monomer for two batch impregnations can fully compound with the fiber preform or the composite preform, and a thermoplastic resin is formed on the surface of the fiber preform, thereby reducing the porosity and improving the performance of the frame.

[0034] Furthermore, in the process of preparing the frame of the present application, the glass fiber plain weave cloth used can better form the frame and has higher mechanical strength. Moreover, since the chemical monomers used can be completely polymerized, no redundant components will be generated and no additional post-processing steps are required.

[0035] In the two dipping processes, by further optimizing the ratio of the monomer solutions injected in the two dipping processes, the balance between the strength in the length direction of the frame and the strength in the direction perpendicular to the length direction can be better coordinated to achieve better frame performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram showing a fiber preform.

[0037] Figure 2 A flow chart and a schematic diagram of the photovoltaic frame preparation method involved in the present application are shown.

[0038] 1: fiber cloth; 2: continuous fiber; 3: fiber felt; 4: yarn guide plate; 5: preheating mechanism; 6: material tank; 7: ultrasonic dispersion device; 8: first glue injection port a; 9: second glue injection port b; 10: frame forming mold; 11: conveying mechanism; 12: cutting mechanism. DETAILED DESCRIPTION

[0039] The following embodiments of the present application are only used to illustrate the specific embodiments of the present application, and these embodiments cannot be understood as limiting the present application. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present application are deemed to be equivalent replacement methods and fall within the scope of protection of the present application.

[0040] The specific embodiments of the present application will be described in more detail below. However, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to enable the scope of the present application to be fully communicated to those skilled in the art.

[0041] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" is an open term, so it should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the implementation of the present application, but the description is based on the general principles of the specification and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.

[0042] As used in this specification, "a" or "an" may mean one or more. As used in the claims, when used with the word "comprising", the word "a" or "an" may mean one or more than one.

[0043] The term "or" is used in the claims to mean "and / or" unless explicitly stated to refer only to alternatives or the alternatives are mutually exclusive, although the present disclosure supports a definition referring only to alternatives and "and / or." As used herein, "another" may mean at least a second or more.

[0044] The present application provides a method for preparing a thermoplastic composite photovoltaic frame, which includes the following steps: using continuous fibers and fiber mats to form a fiber preform; introducing the fiber preform into a mold; injecting a monomer solution into the mold at a low temperature to impregnate the fiber preform once, introducing a fiber cloth at a high temperature to cover the surface of the fiber preform impregnated once to form a composite preform, injecting a monomer solution into the mold to impregnate the fiber cloth of the composite preform twice, polymerizing the monomers in the composite preform impregnated twice at a polymerization temperature, and cooling and processing the fiber preform that has been polymerized to obtain a photovoltaic frame. The present application performs two batch impregnations and integrated reaction pultrusion molding on the preform composed of continuous fibers, fiber mats and fiber cloth, thereby improving the mechanical properties and pultrusion speed of the thermoplastic composite frame. The present application solves the problems in the prior art that the lateral strength and stiffness are poor, the process cost is high, and the conventional impregnation cannot fully impregnate the mesh cloth. The composite photovoltaic frame prepared by the method of the present application is low in cost, easy to recycle, has high toughness, and is easy to repair.

[0045] The present application does not impose any limitation on the impregnation method, and those skilled in the art can implement the impregnation as required, as long as the requirements are met. In the present application, conventional impregnation devices and impregnation means can be used for impregnation, and only the ingredients need to be adjusted as required and impregnated twice.

[0046] In some embodiments of the present application, the temperature range of the low temperature is 80° C. to 170° C.; for example, the temperature of the low temperature can be 80° C., 90° C., 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C. or any range therebetween. Those skilled in the art can select a suitable low temperature according to the monomers and reaction system selected for polymerization.

[0047] In some embodiments of the present application, the temperature range of the high temperature is 120° C. to 180° C.; for example, the temperature of the high temperature can be 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C. or any range therebetween. Those skilled in the art can select a suitable high temperature according to the monomers and reaction system selected for polymerization.

[0048] In some embodiments of the present application, the polymerization temperature ranges from 140° C. to 245° C.; for example, the polymerization temperature may be 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., 200° C., 210° C., 220° C., 230° C., 240° C., 245° C., or any range therebetween. Those skilled in the art may select a suitable polymerization temperature based on the monomers and reaction system selected for polymerization.

[0049] In the present application, those skilled in the art can fully understand that low temperature and high temperature are relative, that is, based on the type of monomer used, those skilled in the art can select the corresponding low temperature and high temperature, as long as the impregnation process can be completed in two stages.

[0050] In some embodiments of the present application, before being introduced into the frame forming mold, the fiber preform is further preheated, preferably at a temperature ranging from 90° C. to 180° C. For example, the preheating temperature may be 90° C., 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C. or any range therebetween.

[0051] In one embodiment of the present application, the low temperature is 80-100°C, such as 90°C, the high temperature is 120-140°C, such as 130°C, and the polymerization temperature ranges from 140-160°C, such as 150°C.

[0052] In one embodiment of the present application, the low temperature is 160-170°C, such as 165°C, the high temperature is 170-180°C, such as 175°C, and the polymerization temperature ranges from 180-245°C, such as 200°C.

[0053] In the present application, the settings of the low temperature, high temperature and polymerization temperature can be adjusted according to the actual process parameters. For example, the low temperature, high temperature and polymerization temperature can be adjusted according to the selected raw materials, so that the internal unidirectional fiber can be better impregnated under low temperature conditions, and the secondary impregnation and curing of the thermoplastic resin can be carried out under high temperature conditions.

[0054] The present application does not impose any limitation on the above temperature control methods, such as placing the entire device in an external constant temperature device or other methods, such as controlling the temperature through a temperature control system. The present application controls the temperature of each stage so that the overall process is in a stable state and the continuous preparation process is achieved, thereby realizing the efficient preparation of photovoltaic frames using thermoplastic composite materials.

[0055] In some embodiments of the present application, the mold includes a low temperature zone and a high temperature zone in sequence in the direction of fiber cloth transportation, and the primary impregnation and the secondary impregnation are carried out in the low temperature zone and the high temperature zone, respectively. The low temperature zone mainly serves to provide a low temperature so as to better impregnate the internal unidirectional fibers, and the high temperature zone mainly serves to provide a high temperature so as to better achieve secondary impregnation and curing of the thermoplastic resin. Using monomers for two batch impregnations can be fully compounded with the fiber preform or the composite preform, and ultimately reduce the porosity of the formed frame profile, improve the frame performance, and improve the strength of the composite frame in the direction perpendicular to the fibers. The outer surface of the frame and the inner cavity surface need to be coated with fiber woven cloth and fiber felt for reinforcement. This overcomes the defect that it is difficult to fully penetrate the fiber preform by impregnating the fiber woven cloth with a monomer solution that forms a thermoplastic resin once.

[0056] In some embodiments of the present application, the volume ratio of the mixture used in the first dipping and the mixture used in the second dipping ranges from (70 to 90): (30 to 10). For example, the volume ratio of the mixture used in the first dipping and the mixture used in the second dipping can be 70:30, 71:29, 72:28, 73:27, 74:26, 75:25, 76:24, 77:23, 78:22, 79:21, 80:20, 81:19, 82:18, 83:17, 84:16, 85:15, 86:14, 87:13, 88:12, 89:11, 90:10 or any range therebetween. In the two dipping processes, by further optimizing the ratio of the monomer solution injected in the two dippings, the balance between the strength in the length direction of the frame and the strength in the direction perpendicular to the length direction can be better coordinated to achieve a more excellent frame performance. The applicant has made a lot of optimizations and found that the volume ratio of the mixture used in the first dipping and the mixture used in the second dipping is maintained within a certain range, so that the final product has excellent performance, for example, excellent overall mechanical properties, excellent strength in the length direction of the frame, and good strength in the direction perpendicular to the length direction. Otherwise, either the strength in the length direction of the frame is poor, or the strength in the direction perpendicular to the length direction is poor, or the overall performance is poor.

[0057] In some embodiments of the present application, the step of forming a fiber preform using continuous fibers and fiber mats includes: arranging and shaping the continuous fibers, introducing fiber mats into the inner surface of the shaped cavity to cover the continuous fibers to form a fiber preform.

[0058] In the present application, the glass fiber plain weave fabric used can better form the frame and has higher mechanical strength. Moreover, since the chemical monomers used can be completely polymerized, no redundant components will be generated and no additional post-processing steps are required.

[0059] In some embodiments of the present application, cooling and processing the fiber preform to obtain a photovoltaic frame includes the following steps: cooling the fiber preform that has completed the polymerization reaction to obtain a frame profile; cutting the frame profile to obtain a fixed-length profile, and performing online polishing and painting on the fixed-length profile to obtain a photovoltaic frame. For example, the cutting is achieved by cutting the structure.

[0060] The present application has no special restrictions on the heat forming and curing, and those skilled in the art can determine it according to the selected chemical monomers, reaction aids and fillers. Those skilled in the art can select the frame profile mold as needed, and the present application has no special restrictions on this. The length, cross-sectional shape, etc. of the frame profile can be determined by those skilled in the art according to the shape and size of the solar cell, and the present application also has no special restrictions.

[0061] In the present application, there is no limitation on the cooling and processing of the fiber preform, as long as those skilled in the art can know and meet the requirements of the present application.

[0062] In some embodiments of the present application, the monomer solution includes: a chemical monomer, a reaction aid and a filler; the chemical monomer is selected from one or more of caprolactam, butyrolactam, valerolactam, undecanolactam, laurolactam or tridecanolactam; or the reaction aid is selected from one or more of an initiator, a catalyst, and a release agent; or the filler is selected from one or more of hollow glass microspheres, calcium carbonate, talc, montmorillonite, titanium dioxide or wollastonite. Among them, the initiator is selected from alkali metals, alkali metal hydrides, alkali metal hydroxides, alkali metal amides or organometallic compounds, preferably the initiator is sodium caprolactam (C10) or caprolactam magnesium bromide (C1); or the catalyst is selected from acyl chlorides or isocyanates, preferably the catalyst is hexamethylenediaminocaprolactam (C20), toluene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI); or the release agent is selected from phosphates, lecithin, stearates or triethanolamine oil, preferably the release agent is zinc stearate.

[0063] The mass ratio of the chemical monomer mixture consisting of the chemical monomer, the reaction aid and the filler to the fiber molding is 2:8 or 3:7.

[0064] In some embodiments of the present application, injecting the monomer solution includes the following steps: mixing chemical monomers, reaction aids and fillers from different material tanks through a high-pressure injection head, and injecting the mixture into the mold after uniformly dispersing the mixture through ultrasonic dispersion. Ultrasonic dispersion treatment can make the various parts mixed and dispersed more uniformly.

[0065] In some embodiments of the present application, when the chemical monomer is caprolactam, butyrolactam or valerolactam, the temperature range of the low temperature is 80°C to 100°C, the temperature range of the high temperature is 120°C to 140°C, the polymerization temperature range is 140°C to 160°C, and the preheating temperature is 90°C to 100°C; for example, the temperature of the low temperature can be 80°C, 85°C, 90°C, 95°C, 100°C or any range therebetween; the temperature of the high temperature can be 120°C, 125°C, 130°C, 135°C, 140°C or any range therebetween; the polymerization temperature can be 140°C, 145°C, 150°C, 155°C, 160°C or any range therebetween; the preheating temperature can be 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C or any range therebetween.

[0066] In one embodiment of the present application, when the chemical monomer is caprolactam, butyrolactam or valerolactam, the low temperature is 90°C, the high temperature is 130°C, the polymerization temperature is 150°C, and the preheating temperature is 95°C.

[0067] In some embodiments of the present application, when the chemical monomer is undecanoic acid tam, lauryl lactam or tridecanolactam, the temperature range of the low temperature is 160°C to 170°C, the temperature range of the high temperature is 170°C to 180°C, the polymerization temperature range is 180°C to 245°C, and the preheating temperature is 170°C to 180°C; for example, the temperature of the low temperature can be 160°C, 161°C, 162°C, 163°C, 164°C, 165°C, 166°C, 167°C, 168°C, 169°C, 170°C or any range therebetween; the temperature of the high temperature can be 170°C, 171°C, 172°C, ℃, 173 ℃, 174 ℃, 175 ℃, 176 ℃, 177 ℃, 178 ℃, 179 ℃, 180 ℃ or any range therebetween; the polymerization temperature may be 180 ℃, 185 ℃, 190 ℃, 195 ℃, 200 ℃, 205 ℃, 210 ℃, 215 ℃, 220 ℃, 225 ℃, 230 ℃, 235 ℃, 240 ℃, 245 ℃ or any range therebetween; the preheating temperature may be 170 ℃, 171 ℃, 172 ℃, 173 ℃, 174 ℃, 175 ℃, 176 ℃, 177 ℃, 178 ℃, 179 ℃, 180 ℃ or any range therebetween.

[0068] In one embodiment of the present application, when the chemical monomer is undecanoic acid tam, lauryl lactam or tridecanolactam, the low temperature range is 165°C, the high temperature range is 175°C, the polymerization temperature range is 200°C, and the preheating temperature is 175°C.

[0069] In some embodiments of the present application, the continuous fiber is selected from one or more of glass fiber roving, polymer fiber or biomass fiber, preferably the polymer fiber is selected from ultra-high molecular weight polyethylene, polyethylene terephthalate, poly(p-phenylene phthalamide), preferably the biomass fiber is selected from bamboo pulp fiber, hemp pulp fiber and chitosan fiber; the fiber felt is selected from carbon fiber felt, glass fiber felt or polyester fiber felt; or the fiber cloth is selected from glass fiber plain weave cloth, glass fiber twill weave cloth, glass fiber satin weave cloth.

[0070] A device for preparing a thermoplastic composite photovoltaic frame for implementing the above method, such as Figure 2 As shown, it includes: a fiber preform forming mechanism, which uses continuous fibers and fiber mats to form a fiber preform; a frame forming mold 10, which is used to place the fiber preform and can control the temperature and is used for impregnation and polymerization of the fiber preform; a glue injection mechanism, which can inject a monomer solution into the mold; a conveying mechanism 11 and a cutting mechanism 12, which are used to convey the cooled frame to form and process it into a photovoltaic frame; wherein the mold is divided into a low-temperature zone and a high-temperature zone, the glue injection mechanism includes a primary impregnation injection channel and a secondary impregnation injection channel, the low-temperature zone is connected to the primary impregnation injection channel for primary impregnation, and the high-temperature zone is connected to the secondary impregnation injection channel for secondary impregnation. In the low temperature zone of the mold, a monomer solution is injected into the mold through a primary impregnation injection channel and a first injection port 8 to perform a primary impregnation on the fiber preform. In the high temperature zone of the mold, a fiber cloth is introduced into the mold to cover the surface of the fiber preform that has been impregnated once to form a composite preform. A monomer solution is injected into the mold through a secondary impregnation injection channel and a second injection port 9 to perform a secondary impregnation on the fiber cloth of the composite preform. In the high temperature zone of the mold, the monomer in the composite preform that has been impregnated twice is polymerized in the injection mechanism mold; wherein the primary impregnation injection channel and the secondary impregnation injection channel are independent of each other.

[0071] The present application provides a device for preparing a thermoplastic composite photovoltaic frame, such as Figure 2As shown, it includes: a fiber preform forming mechanism, which uses continuous fibers and fiber mats to form a fiber preform; a frame forming mold 10, which is used to place the fiber preform and can control the temperature and is used to perform impregnation and polymerization reactions of the fiber preform; a glue injection mechanism, which can inject a monomer solution into the mold; a conveying mechanism 11 and a cutting mechanism 12, which are used to convey the cooled frame to form and process it into a photovoltaic frame; wherein the mold is divided into a low temperature zone and a high temperature zone, and the glue injection mechanism includes a primary impregnation injection channel and a secondary impregnation injection channel, the low temperature zone is connected to the primary impregnation injection channel for primary impregnation, and the high temperature zone is connected to the secondary impregnation injection channel for secondary impregnation. Through this device, two batch impregnations of the chemical monomer mixture can be achieved, which can be fully compounded with the fiber preform, reduce the porosity, and improve the performance of the frame.

[0072] like Figure 2 As shown, in the low temperature zone of the mold, a monomer solution is injected into the mold through the primary impregnation injection channel and the first injection port 8 to impregnate the fiber preform once, in the high temperature zone of the mold, a fiber cloth is introduced into the mold to cover the surface of the fiber preform impregnated once to form a composite preform, and a monomer solution is injected into the mold through the secondary impregnation injection channel and the second injection port 9 to impregnate the fiber cloth of the composite preform twice, in the high temperature zone of the mold, the monomer in the composite preform impregnated twice is polymerized in the injection mechanism mold; wherein the primary impregnation injection channel and the secondary impregnation injection channel are independent of each other. The low temperature zone is mainly used for impregnation of the internal unidirectional fibers, and the high temperature zone is used for impregnation and curing of the secondary resin. Through the cooperation of the low temperature zone and the high temperature zone, it is possible to better coordinate the balance between the strength in the length direction of the frame and the strength in the direction perpendicular to the length direction, and achieve a more excellent frame performance.

[0073] like Figure 2 As shown, the glue injection mechanism sequentially comprises a material tank 6, an ultrasonic dispersion device 7, a first glue injection port 8, and a second glue injection port 9. The glue injection mechanism can better cooperate with the two batch impregnations of the chemical monomer mixture.

[0074] In some embodiments of the present application, the device further includes a temperature control system, which can control the temperature of the mold based on the different monomers used for impregnation and polymerization, and can independently control the mold within the following temperature ranges: the low temperature range is 80°C to 170°C, or the high temperature range is 120°C to 180°C, or the polymerization temperature range is 140°C to 245°C. Moreover, by controlling the temperature of the two batch impregnations, an efficient polymerization reaction can be achieved, so that the polymerization reaction is more sufficient, the monomer can be fully compounded with the fiber preform, the porosity is reduced, and the frame performance is improved. The value of the low temperature temperature, the high temperature temperature, or the polymerization temperature is described above.

[0075] In some embodiments of the present application, the device further includes a preheating mechanism 5, which is used to preheat the fiber preform before being introduced into the frame forming mold, and preferably the temperature control system controls the preheating temperature of the preheating mechanism to be 90° C. to 180° C. Through the preheating treatment of the preheating mechanism 5, impregnation can be better achieved. The specific value of the preheating temperature of the preheating mechanism controlled by the temperature control system is described above.

[0076] In some embodiments of the present application, the injection mechanism controls the volume ratio of the mixture entering the primary immersion injection channel and the secondary immersion injection channel to be in the range of (70-90):(30-10). The specific value of the volume ratio of the mixture entering the primary immersion injection channel and the mixture entering the secondary immersion injection channel is described above.

[0077] In some embodiments of the present application, a temperature control system is capable of controlling the temperature of a mold and a preheating mechanism based on different monomers used for impregnation and polymerization reactions, wherein when the chemical monomer is caprolactam, butyrolactam or valerolactam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 80°C to 100°C, the temperature control system controls the temperature range of the high temperature zone to be 120°C to 140°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 140°C to 160°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 90°C to 100°C; when the chemical monomer is undecanoic acid tam, lauryl lactam or tridecanoic acid tam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 160°C to 170°C, the temperature control system controls the temperature range of the high temperature zone to be 170°C to 180°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 80°C to 245°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 170°C to 180°C. For specific values ​​of the temperature in the low temperature zone, the temperature in the high temperature zone, the polymerization temperature, and the preheating temperature, please refer to the above.

[0078] In some embodiments of the present application, the fiber preform forming mechanism includes: a continuous fiber arranging mechanism for arranging and shaping continuous fibers; a fiber preform forming mechanism for introducing fiber felt into the inner cavity surface of the shaping to cover the continuous fibers to form a fiber preform.

[0079] like Figure 2 As shown, the device also includes an ultrasonic dispersion device 7. The present application uses an ultrasonic dispersion device to perform ultrasonic dispersion treatment to make the filler more evenly dispersed.

[0080] Use Figure 2 The device described above realizes the preparation of the thermoplastic composite photovoltaic frame as follows:

[0081] The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and is introduced into the glass fiber chopped strand mat 3 to the inner surface of the shape (see Figure 1 The fiber preform is covered with the surface covered by the reference numeral 3) to form a fiber preform, which is preheated by the preheating mechanism 5 and then introduced into the frame forming mold 10;

[0082] Chemical monomers, initiators, catalysts, release agents, and fillers are introduced into different material tanks, and the above materials are mixed by a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly by an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then Figure 2 The first injection port 8 shown is injected into the impregnation cavity of the low temperature zone of the mold. The chemical monomer mixture is fully impregnated into the fiber preform in the impregnation cavity of the low temperature zone of the mold, i.e., a primary impregnation; then, the glass fiber plain woven cloth 1 is introduced into the high temperature zone of the mold to cover the outer surface of the impregnated preform, and the same chemical monomer mixture is simultaneously injected into the impregnation cavity of the high temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth, i.e., a secondary impregnation; the volume ratio of the chemical monomer mixture injected through the first injection port 8 and the chemical monomer mixture injected through the second injection port 9 is controlled to be in the range of (70-90): (30-10), wherein the mass ratio of the chemical monomer mixture to the fiber preform is 2:8; the temperature of the high temperature zone is increased to the polymerization temperature, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed length profile, which is polished and coated with fluorocarbon coating online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0083] The present application provides a thermoplastic composite photovoltaic frame, which includes the following structures stacked in sequence: a fiber molding with a thermoplastic resin formed on the surface, including continuous fibers 2 and fiber felt 3; a fiber cloth 1 with a thermoplastic resin formed on the surface; and a weather-resistant coating coated on the fiber cloth.

[0084] In some embodiments of the present application, the thermoplastic composite photovoltaic frame is made of continuous glass fiber reinforced polyamide 6, and the surface is coated with a weather-resistant water-based polyurethane coating. The polyamide 6 is polymerized by the bio-based chemical monomer caprolactam during the frame preparation process, and the caprolactam is fermented from biomass raw materials such as straw, sugar cane, and vegetable oil; the continuous fiber can also be one or more of carbon fiber, polymer fiber, and biomass fiber; the surface weather-resistant coating can also be fluorocarbon coating and fluorourethane coating; the bio-based chemical monomer can also be one or more of butyrolactam, valerolactam, undecanoic acid, lauryl lactam, and tridecanoic acid.

[0085] In some embodiments of the present application, the thermoplastic resin is obtained by polymerizing a monomer solution including chemical monomers, reaction aids and fillers on a fiber molding. The monomers of the chemical monomers, reaction aids and fillers are described above.

[0086] In some embodiments of the present application, the thermoplastic composite photovoltaic frame is prepared by the above method, or prepared by the above device.

[0087] Example 1

[0088] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0089] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0090] Subsequently, a 100-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0091] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 7:3, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0092] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed length profile, which is polished and coated with fluorocarbon coating online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0093] Example 2

[0094] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0095] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0096] Subsequently, a 100-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0097] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 8:2, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0098] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0099] Example 3

[0100] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0101] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0102] Subsequently, a 100-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0103] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 9:1, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0104] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0105] Example 4

[0106] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0107] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0108] Subsequently, a 100-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0109] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 6:4, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0110] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0111] Example 5

[0112] Use Figure 2 The glass fiber roving 2 on the creel is arranged and molded through the yarn guide plate 4, and the 50-gram glass fiber chopped strand mat 3 is introduced into the inner cavity surface of the mold (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0113] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0114] Subsequently, a 50-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0115] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 7:3, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0116] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0117] Example 6

[0118] Use Figure 2 The glass fiber roving 2 on the creel is arranged and molded through the yarn guide plate 4, and the 50-gram glass fiber chopped strand mat 3 is introduced into the inner cavity surface of the mold (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0119] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0120] Subsequently, a 50-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0121] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 8:2, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0122] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0123] Example 7

[0124] Use Figure 2 The glass fiber roving 2 on the creel is arranged and molded through the yarn guide plate 4, and the 50-gram glass fiber chopped strand mat 3 is introduced into the inner cavity surface of the mold (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0125] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0126] Subsequently, a 50-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0127] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 9:1, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0128] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0129] Example 8

[0130] Use Figure 2 The glass fiber roving 2 on the creel is arranged and molded through the yarn guide plate 4, and the 50-gram glass fiber chopped strand mat 3 is introduced into the inner cavity surface of the mold (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0131] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0132] Subsequently, a 50-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 130°C.

[0133] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 6:4, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0134] The temperature of the high temperature zone is raised to 150°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0135] Example 9

[0136] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 175° C.) and then introduced into a frame forming mold 10.

[0137] Undecanoic acid amide as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 165°C at this time.

[0138] Subsequently, a 100-gram glass fiber plain woven cloth 1 is introduced into the high-temperature zone of the mold to cover the outer surface of the preform after impregnation, and the same chemical monomer mixture mentioned above is simultaneously injected into the impregnation cavity of the high-temperature zone of the mold through the second injection port 9 to fully impregnate the glass fiber cloth. At this time, the temperature of the high-temperature zone is 175°C.

[0139] In this embodiment, the volume ratio of the chemical monomer mixture injected through the first injection port 8 to the chemical monomer mixture injected through the second injection port 9 is 8:2, wherein the mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0140] The temperature of the high temperature zone is raised to 200°C, so that the fully impregnated preform is further fully polymerized in the high temperature zone of the mold, and finally cooled and shaped in the cooling zone of the mold to obtain a frame profile; the frame profile is cut by a cutting device to obtain a fixed-length profile, and the fixed-length profile is coated with fluorocarbon coating and polished and painted online to obtain a photovoltaic frame. The mechanical strength of the photovoltaic frame is tested using a universal testing machine.

[0141] Comparative Example 1

[0142] Use Figure 2 The device shown in the figure is used for production. The glass fiber roving 2 on the creel is arranged and shaped by the yarn guide plate 4, and the glass fiber chopped strand mat 3 with a weight of 100 grams is introduced to the inner cavity surface of the shape (see Figure 1 The surface covered by the reference numeral 3 in the figure is covered to form a fiber preform, which is preheated by a preheating mechanism 5 (the preheating temperature is 95° C.) and then introduced into a frame forming mold 10.

[0143] Caprolactam as a chemical monomer, sodium caprolactam as an initiator, hexamethylenediaminocaprolactam as a catalyst, zinc stearate as a release agent, and hollow glass microspheres as a filler are introduced through different material tanks, and the above materials are mixed through a high-pressure injection mixing head to obtain a chemical monomer mixture, which is further dispersed uniformly through an ultrasonic dispersion mechanism 7 to obtain a chemical monomer mixture, and then through Figure 2 The first injection port 8 shown is injected into the low temperature zone impregnation cavity of the mold. The chemical monomer mixture fully impregnates the fiber preform in the low temperature zone impregnation cavity of the mold, and the temperature of the low temperature zone is 90°C at this time.

[0144] Then, a glass fiber plain woven cloth 1 with a weight of 100 grams is introduced into the high temperature zone of the mold to cover the outer surface of the impregnated preform.

[0145] In the comparative example, all the chemical monomer mixture is injected through the first injection port 8. The mass ratio of the chemical monomer mixture to the fiber molding is 2:8.

[0146] The temperature of the high temperature zone was increased to 150°C, so that the fully impregnated preform was further polymerized in the high temperature zone of the mold. However, due to incomplete impregnation, full polymerization could not be achieved, and the strength of the formed material was poor, and ultimately it could not be effectively processed into a profile.

[0147] Table 1

[0148]

[0149]

[0150] Symbol definition:

[0151] ○Indicates that the mechanical properties tested by a universal testing machine are generally excellent

[0152] ◎Indicates that the mechanical properties tested by a universal testing machine are excellent, but the strength in the length direction of the frame is slightly weaker, but the strength in the direction perpendicular to the length direction is slightly stronger

[0153] △ indicates that the mechanical properties tested by the universal testing machine are average, but the strength in the length direction of the frame is poor, but the strength in the direction perpendicular to the length direction is strong

[0154] Although the embodiments of the present application are described above, the present application is not limited to the above specific embodiments and application fields, and the above specific embodiments are merely illustrative and instructive, rather than restrictive. A person of ordinary skill in the art can make many forms under the guidance of this specification and without departing from the scope of protection of the claims of the present application, all of which belong to the protection of the present application.

Claims

1. A method for preparing a thermoplastic composite photovoltaic frame, wherein The following steps are involved: forming a fiber preform using continuous fibers and fiber mats; introducing the fiber preform into a mold; At low temperature, injecting a monomer solution into the mold to impregnate the fiber preform once, At high temperature, a fiber cloth is introduced to cover the surface of the fiber preform that has been impregnated once to form a composite preform, and the monomer solution is injected into the mold to perform secondary impregnation on the fiber cloth of the composite preform. At the polymerization temperature, the monomers in the composite preform that has been impregnated twice are polymerized, and the fiber preform that has been polymerized is cooled and processed to obtain a photovoltaic frame.

2. The method according to claim 1, in, The low temperature range is 80°C to 170°C, or The high temperature range is 120°C to 180°C, or The polymerization temperature ranges from 140°C to 245°C.

3. The method according to claim 1 or 2, in, Before being introduced into the frame forming mold, the method further comprises preheating the fiber preform, wherein the preheating temperature ranges preferably from 90°C to 180°C.

4. The method according to any one of claims 1 to 3, in, The mold includes a low temperature zone and a high temperature zone in sequence in the direction of transporting the fiber cloth, and the primary impregnation and the secondary impregnation are respectively performed in the low temperature zone and the high temperature zone.

5. The method according to any one of claims 1 to 4, in, The volume ratio of the mixture used in the first impregnation to the mixture used in the second impregnation is in the range of (70-90):(30-10).

6. The method according to any one of claims 1 to 5, in, The step of forming a fiber preform using continuous fibers and fiber mats includes: arranging and shaping the continuous fibers, introducing fiber mats into the inner cavity surface of the shaping to cover the continuous fibers to form a fiber preform.

7. The method according to any one of claims 1 to 6, in, Cooling and processing the fiber preform to obtain a photovoltaic frame includes the following steps: Cooling the fiber preform that has completed the polymerization reaction to obtain a frame profile; The frame profile is cut to obtain a fixed-length profile, and the fixed-length profile is polished and painted online to obtain a photovoltaic frame.

8. The method according to any one of claims 1 to 7, in, The monomer solution includes: chemical monomers, reaction aids and fillers; Injecting the monomer solution comprises the following steps: mixing chemical monomers, reaction aids and fillers from different material tanks through a high-pressure injection head, and uniformly dispersing the mixture through ultrasonic dispersion before injecting it into the mold.

9. The method according to claim 8, in, The chemical monomer is selected from one or more of caprolactam, butyrolactam, valerolactam, undecanolactam, laurolactam or tridecanolactam; or The reaction aid is selected from one or more of an initiator, a catalyst, and a release agent; or The filler is selected from one or more of hollow glass microspheres, calcium carbonate, talcum powder, montmorillonite, titanium dioxide or wollastonite.

10. The method according to claim 9, in, When the chemical monomer is caprolactam, butyrolactam or valerolactam, the low temperature ranges from 80°C to 100°C, the high temperature ranges from 120°C to 140°C, the polymerization temperature ranges from 140°C to 160°C, and the preheating temperature is from 90°C to 100°C; When the chemical monomer is undecanoic acid, lauryl lactam or tridecanolactam, the low temperature ranges from 160°C to 170°C, the high temperature ranges from 170°C to 180°C, the polymerization temperature ranges from 180°C to 245°C, and the preheating temperature is 170°C to 180°C.

11. The method according to any one of claims 1 to 10, in, The continuous fiber is selected from one or more of glass fiber roving, polymer fiber or biomass fiber, preferably the polymer fiber is selected from ultra-high molecular weight polyethylene, polyethylene terephthalate, poly(p-phenylene phthalamide), and the biomass fiber is selected from bamboo pulp fiber, hemp pulp fiber and chitosan fiber; The fiber felt is selected from carbon fiber felt, glass fiber felt or polyester fiber felt; or, The fiber cloth is selected from glass fiber plain woven cloth, glass fiber twill woven cloth, and glass fiber satin woven cloth.

12. A device for preparing a thermoplastic composite photovoltaic frame, include: A fiber preform forming mechanism, which forms a fiber preform using continuous fibers and fiber mats; A frame forming mold, which is used to place the fiber preform and can control the temperature and is used to perform impregnation and polymerization reactions of the fiber preform; A glue injection mechanism capable of injecting a monomer solution into the mold; A conveying mechanism and a cutting mechanism, which are used to convey the cooled frame and process it into a photovoltaic frame; Among them, the mold is divided into a low-temperature zone and a high-temperature zone, and the glue injection mechanism includes a primary dipping injection channel and a secondary dipping injection channel. The low-temperature zone is connected to the primary dipping injection channel for the primary dipping, and the high-temperature zone is connected to the secondary dipping injection channel for the secondary dipping.

13. The preparation device according to claim 12, in, In the low temperature area of ​​the mold, the monomer solution is injected into the mold through a primary impregnation injection channel and a first injection port to perform a primary impregnation on the fiber preform. In the high temperature zone of the mold, a fiber cloth is introduced into the mold to cover the surface of the fiber preform that has been impregnated once to form a composite preform, and the monomer solution is injected into the mold through a secondary impregnation injection channel and a second injection port to perform secondary impregnation on the fiber cloth of the composite preform. In the high temperature area of ​​the mold, the monomers in the composite preform that has been impregnated twice are polymerized in the injection mechanism mold; The primary impregnation injection flow channel and the secondary impregnation injection flow channel are independent of each other.

14. The manufacturing apparatus according to claim 13, further comprising a temperature control system capable of controlling the temperature of the mold based on the difference in monomers used for impregnation and polymerization, and capable of independently controlling the mold within the following temperature ranges: The low temperature range is 80°C to 170°C, or The high temperature range is 120°C to 180°C, or The polymerization temperature ranges from 140°C to 245°C.

15. The preparation device according to claim 13 or 14, further comprising: include: A preheating mechanism is used to preheat the fiber preform before it is introduced into the frame forming mold. Preferably, the temperature control system controls the preheating temperature of the preheating mechanism to be 90°C to 180°C.

16. The preparation device according to any one of claims 13 to 15, in, The glue injection mechanism controls the volume ratio of the mixture entering the primary dipping injection channel and the mixture entering the secondary dipping injection channel to be in the range of (70-90):(30-10).

17. The preparation device according to claim 14 or 15, further comprising: include: A temperature control system capable of controlling the temperature of the mold and preheating mechanism based on the monomers used for impregnation and polymerization, When the chemical monomer is caprolactam, butyrolactam or valerolactam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 80°C to 100°C, the temperature control system controls the temperature range of the high temperature zone to be 120°C to 140°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 140°C to 160°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 90°C to 100°C; When the chemical monomer is undecanoic acid, lauryl lactam or tridecanolactam, the temperature control system controls the temperature range of the low temperature zone of the injection mechanism to be 160°C to 170°C, the temperature control system controls the temperature range of the high temperature zone to be 170°C to 180°C, the temperature control system controls the polymerization temperature range of the high temperature zone to be 80°C to 245°C, and the temperature control system controls the preheating temperature of the preheating mechanism to be 170°C to 180°C.

18. A thermoplastic composite photovoltaic frame, comprising the following structure stacked in sequence: A fiber molded body including continuous fibers and fiber mats having a thermoplastic resin formed on the surface; A fiber cloth having a thermoplastic resin formed on the surface; and A weather-resistant coating is coated on the fiber cloth.

19. The photovoltaic frame according to claim 18, in, The thermoplastic resin is obtained by polymerizing a monomer solution including chemical monomers, reaction aids and fillers on a fiber molding.

20. The photovoltaic frame according to claim 18 or 19, in, It is prepared by the method according to any one of claims 1 to 12 or by the preparation device according to any one of claims 13 to 17.

Citation Information

Patent Citations

  • Pultrusion profile for photovoltaic module frame, photovoltaic module frame and preparation method

    CN115625909A

  • Preparation method and equipment of fiber reinforced composite material

    CN117021620A

  • Solar cell panel composite material frame pultrusion equipment and pultrusion process

    CN118144324A

  • Co-extrusion equipment for weather-resistant composite material profile

    CN221292363U

Cited By

  • Continuous fiber reinforced thermoplastic multilayer composite material and forming method and device thereof

    CN120171080A