Low-temperature sealing-starting high-temperature-resistant water-blocking PE film and preparation method thereof

The PE film prepared by five-layer co-extrusion, combined with barrier masterbatch of specific polymers and nanocellulose fibers, solves the problems of insufficient barrier properties and difficulty in recycling of PE film, and achieves low-temperature sealing, high heat resistance and excellent water and oxygen barrier properties.

CN119036976AActive Publication Date: 2024-11-29QINGDAO DONGHAI PACKAGING IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411233875.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Existing PE films are insufficient in blocking oxygen and water vapor, and their multi-layered composite structure makes recycling difficult, making it hard to meet the demands for high-quality products and environmental protection requirements.

Method used

PE film is prepared by five-layer co-extrusion. The inner layer is a mixture of low-density polyethylene and linear low-density polyethylene, with PPA additives and opening agents added to reduce heat sealing temperature and improve lubricity. HDPE is added to the second inner layer, middle layer and second outer layer to improve density and barrier properties. The outer layer uses a combination of high-density and low-density HDPE and LLDPE, and barrier masterbatch prepared by adding oxidized nanocellulose filaments and aramid fibers to form multiple hydrogen bonds and a three-dimensional network structure to enhance barrier ability.

Benefits of technology

It achieves low-temperature sealing, high heat resistance, and excellent water and oxygen barrier properties, reducing heat sealing damage to the membrane, improving recycling rate, and enhancing the membrane's mechanical strength and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027133310000081
    Figure BDA0005027133310000081
  • Figure BDA0005027133310000091
    Figure BDA0005027133310000091
  • Figure BDA0005027133310000101
    Figure BDA0005027133310000101
Patent Text Reader

Abstract

The invention relates to the field of high polymer materials, and particularly discloses a low-temperature sealing-starting high-temperature-resistant water-blocking PE film and a preparation method thereof. The PE film sequentially comprises an inner layer, a secondary inner layer, a middle layer, a secondary outer layer and an outer layer from inside to outside, the inner layer is prepared from the following raw materials: LDPE, LLDPE, MLLDPE, a PPA auxiliary agent, a slipping agent and an anti-blocking agent; the secondary inner layer is prepared from the following raw materials: HDPE (high-density polyethylene), barrier master batch and a PPA (Phenyl- The middle layer is prepared from the following raw materials: HDPE (high-density polyethylene), barrier master batches and a PPA (Phenyl The secondary outer layer is prepared from the following raw materials: HDPE, barrier master batches and a PPA auxiliary agent; the outer layer is prepared from the following raw materials: LLDPE, MLLDPE, HDPE, barrier master batch, a PPA auxiliary agent and an antioxidant. The PE film is made of a single material, is convenient to recycle, and is good in water resistance and oxygen resistance, high in temperature resistance, small in thermal shrinkage rate, low in initial sealing temperature and high in heat sealing strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and more specifically, to a low-temperature sealing, high-temperature-resistant and water-resistant PE film and a preparation method thereof. Background Art

[0002] In recent years, plastic packaging materials have mainly developed in the direction of high barrier, non-toxic, anti-aging, high strength, co-extruded film, composite film, and environmentally friendly. Polyethylene is the simplest macromolecular organic compound and one of the most widely used macromolecular materials in the world today. The raw materials are formed by blending, injection, extrusion and blow molding, and are widely used in industry and agriculture, food packaging and daily life. PE is a polymer formed by the polymerization of ethylene monomers. It is a typical thermoplastic plastic and is an odorless, tasteless, non-toxic combustible white powder. Factors such as the crystallinity and relative molecular mass of PE have a certain influence on its physical and mechanical properties. It has excellent mechanical properties, good water vapor barrier properties, high impact strength, light weight and good printing properties. However, PE materials also have shortcomings. The barrier properties to oxygen are poor and cannot well prevent the penetration of oxygen in the external environment. Therefore, research on how to improve the barrier properties of PE films is the focus of current research in the field of PE film technology.

[0003] At present, in order to improve the barrier properties of PE films in the market, composite structures are mostly used, such as PET / PE, BOPP / PE, PA / PE, KPET / PE or three-layer structures PET / PA / PE, BOPP / PA / PE. PE composite films made of multiple materials are cumbersome and difficult to sort and classify during recycling, and the recycling rate is low. Influenced by environmental protection policies and the concept of sustainable development, the use of single materials for plastic packaging materials has received increasing attention. Under the premise of ensuring the performance requirements of packaging, it has become a consensus for the healthy development of the industry to use a single material as much as possible to facilitate recycling. However, PE single-material films mostly use PE / PE material structure, and both layers are ordinary polyethylene resins. The moisture barrier and oxygen barrier properties cannot meet the needs of high-quality products. Summary of the invention

[0004] In order to improve the water and oxygen barrier properties of polyethylene and meet the recycling requirements of a single material, the present application provides a low-temperature sealing and high-temperature-resistant water-barrier PE film and a preparation method thereof.

[0005] In the first aspect, the present application provides a low-temperature sealing high temperature-resistant water-resistant PE film, which adopts the following technical solution: a low-temperature sealing high temperature-resistant water-resistant PE film, which includes the following five layers from the inside to the outside: an inner layer, a sub-inner layer, an intermediate layer, a sub-outer layer and an outer layer; The inner layer comprises the following raw materials in parts by weight: 8-12 parts of LDPE, 25-35 parts of LLDPE, 55-65 parts of MLLDPE, 0.6-1 parts of PPA additive, 1.2-2 parts of lubricant, and 5-6 parts of opening agent; The secondary inner layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 1-2 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additive; the middle layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 2.5-3.5 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additive; The secondary outer layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 2-3 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additives; the outer layer comprises the following raw materials in parts by weight: 35-45 parts of LLDPE, 25-35 parts of MLLDPE, 25-35 parts of HDPE, 3.5-4 parts of barrier masterbatch, 0.2-0.6 parts of PPA additives, and 0.2-0.6 parts of antioxidants.

[0006] By adopting the above technical scheme, low-density polyethylene, linear low-density polyethylene and metallocene linear low-density polyethylene are used as the raw materials of the inner layer, and mixed in a certain proportion. While reducing the density of the inner layer, the heat sealing temperature is reduced, the heat sealing property is better provided, the bag making temperature and pressure are reduced, and the damage of the heat sealing to the PE film is reduced to the greatest extent, providing better barrier capacity. In addition, the addition of an opening agent, a slip agent and a PPA additive can improve the antistatic and lubricity, and improve the moisture resistance, significantly reduce the friction coefficient and the bonding resistance, and significantly improve the High film blowing efficiency prevents adhesion of film pieces and agglomeration between pellets, increases the smoothness of the film surface, and reduces dust accumulation; in the sub-inner layer, sub-outer layer, middle layer and outer layer, from outside to inside, the amount of barrier masterbatch is set according to the addition amount of high-low-high-low, thereby playing a zigzag pulse effect and improving the gas barrier property of the film; and HDPE is added to the sub-inner layer, middle layer, sub-outer layer and outer layer to increase the density of the PE film itself, improve the overall temperature resistance and barrier property, and reduce the permeability of water vapor and oxygen.

[0007] Optionally, the inner layer includes MLLDPE with a mass ratio of 1:1.5-2 and a density of 0.915 g / cm 3 , No. 1 MLLDPE with a melt index of 1 g / 10 min and a density of 0.913 g / cm 3 , No. II MLLDPE with a melt index of 2g / 10min.

[0008] By adopting the above technical solution, two kinds of materials with similar density and lower than 0.915g / cm 3MLLDPE has a narrower molecular weight distribution, a higher copolymer content and a more uniform polymer structure, resulting in lower sealing strength and stronger heat sealing strength, while improving the tear strength and puncture resistance of the film.

[0009] Optionally, the HDPE in the secondary inner layer includes a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.950g / cm 3 , No. 2 HDPE with a melt index of 0.9g / 10min; The HDPE in the middle layer has a mass ratio of 1:1.5-2 and a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.956g / cm 3 , No. 3 HDPE with a density of 1g / 10min; The HDPE in the secondary outer layer has a mass ratio of 1:1.5-2 and a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.958g / cm 3 , No. 4 HDPE with a density of 0.28g / 10min.

[0010] By adopting the above technical solution, two types of HDPE based on No. 2 HDPE are added to the sub-inner layer, the middle layer and the sub-outer layer, and the density of the two types of HDPE is 0.95-0.97g / cm 3 In order to increase the overall density of the PE film, improve the temperature resistance and barrier properties of the PE film, reduce the thermal shrinkage rate, and improve the resistance to boiling.

[0011] Optionally, the density of LLDPE in the outer layer is 0.9188 g / cm 3 , melt index is 1.9g / 10min, density of MLLDPE is 0.94g / cm 3 , melt index is 0.9g / 10min, density of HDPE is 0.961g / cm 3 , the melt index is 0.7g / 10min.

[0012] By adopting the above technical scheme, the density of HDPE in the outer layer is higher than the density of No. 2 HDPE, No. 3 HDPE and No. 4 HDPE in the sub-inner layer, the middle layer and the sub-outer layer, which can provide better barrier properties and improve the tear resistance and impact resistance of the PE film. In addition, the HDPE and MLLDPE in the outer layer can cooperate to control the crystallinity and melting point of the outer layer, thereby improving the barrier properties and heat resistance of the PE film and reducing the gas permeation.

[0013] Optionally, the density of LDPE in the inner layer is 0.924 g / cm 3 , melt index is 1.9g / 10min, density of LLDPE is 0.918g / cm 3 , the melt index is 2g / 10min.

[0014] By adopting the above technical solution, LDPE and LLDPE are both polyethylenes with lower density. LLDPE has the characteristics of high impact resistance and good creep resistance at high temperature, and LDPE has good softness, transparency and extensibility, which can reduce the density of the inner layer and improve the barrier capacity.

[0015] Optionally, the preparation method of the barrier masterbatch is as follows: The oxidized nanocellulose fibrils are subjected to ultrasonic dispersion treatment with deionized water for 1-2 hours to prepare a suspension with a concentration of 0.5-1wt%, polyvinyl alcohol is dissolved in deionized water to prepare a polyvinyl alcohol aqueous solution with a concentration of 3.5-4wt%, and aramid fibers are broken into 3-5mm fragments, added to ethanol, ultrasonically removed, and then dissolved to prepare a dispersion with a concentration of 0.5-0.7wt%; The polyvinyl alcohol aqueous solution and the suspension are mixed, stirred evenly, degassed, cast, and dried to obtain a matrix film, wherein the mass ratio of the oxidized nanocellulose fibrils to the polyvinyl alcohol is 1-1.5:1; The base film is immersed and pulled in the dispersion for 3-5 times, and then immersed in a tert-butyl alcohol solution with a concentration of 50-55wt% at 60-70°C for 1-3 minutes, taken out and repeatedly washed with ultrapure water and anhydrous ethanol, freeze-dried, and crushed to obtain an initial powder; the initial powder and No. 1 HDPE are mixed, melted, and granulated at a mass ratio of 0.03-0.06:1.

[0016] By adopting the above technical scheme, the oxidized nanocellulose fibrils are TEMPO-oxidized cellulose nanofibrils, which contain a large number of free hydroxyl groups and carboxyl groups, and polyvinyl alcohol is a long-chain semi-crystalline polymer, and its aqueous solution contains abundant hydroxyl sites. Therefore, the oxidized cellulose nanofibrils and polyvinyl alcohol can form multiple hydrogen bonds. The combination of hydrogen bonds reduces the content of free hydroxyl groups on the molecular chains of both, reduces the surface energy of the base film, inhibits the formation of hydrogen bonds with water droplets, and improves the water barrier. Then, the dispersion formed by aramid fibers is freeze-dried on the base film to form aerogel. Aramid fibers have extremely strong intermolecular forces due to their highly oriented molecular chains, which makes them chemically stable. The strong characteristics of the aramid nanofiber are dissolved in a mixture of potassium hydroxide / dimethyl sulfoxide to obtain aramid nanofibers. The aramid nanofibers are impregnated and deposited on the substrate film. After freeze-drying, aggregates with a layered three-dimensional network structure are formed on the substrate film. The aramid nanofibers have a large number of mesoporous structures, which extend the permeation path of water vapor and oxygen, improve the barrier ability, and have good flexibility and excellent UV protection. The tensile strength of the PE film is improved. Finally, the No. 1 HDPE contained in the sub-inner layer, the middle layer, and the sub-outer layer is used as the base material of the barrier masterbatch to increase the dispersibility and compatibility of the barrier masterbatch in the sub-inner layer, the middle layer, and the sub-outer layer, and reduce the influence of the barrier masterbatch on the mechanical strength of the PE film.

[0017] Optionally, tristearin-modified silica is further added to the dispersion, and the mass ratio of tristearin-modified silica to the aramid fiber in the dispersion is 0.1-0.2:1.

[0018] By adopting the above technical scheme, aramid fiber is made of aromatic polyamide, and its molecular structure contains polar amide groups, so it has a certain polarity. When mixed with No. 1 HDPE and melted, in order to improve its dispersion uniformity with No. 1 HDPE, tristearate-modified silica is added to the dispersion to increase its hydrophobicity, thereby making the surface of the barrier masterbatch hydrophobic, increasing its dispersibility in No. 1 HDPE, and reducing the dispersion and dissolution of water vapor in the aramid aerogel, making it difficult for water vapor to penetrate the barrier masterbatch and diffuse inward, and reducing the porosity of the aramid aerogel, reducing the scattering and refraction of light, and increasing the transparency of the film.

[0019] Optionally, the thickness ratio of the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer is 2-2.5:1-1.5:2.8-3:1-1.5:2-2.5.

[0020] By adopting the above technical solution and adjusting the thickness ratio between the layers, better gas and moisture barrier properties can be provided, and the preservation and protection effects of the PE film can be enhanced. In addition, the inner layer can directly improve the heat sealing strength and uniformity of the heat sealing, while the outer layer can increase the mechanical strength and stiffness of the PE film and improve the barrier strength.

[0021] In the second aspect, the present application provides a method for preparing a low-temperature sealing high temperature-resistant and water-resistant PE film, which adopts the following technical solution: A method for preparing a low-temperature sealing high-temperature-resistant and water-resistant PE film comprises the following steps: The raw materials in the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are respectively mixed evenly to obtain the inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material; The inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material are added into the hopper of the extruder respectively, and the PE film is obtained through extrusion melting, casting, film drawing, blowing, pulling and winding.

[0022] By adopting the above technical scheme, the raw materials of each layer are first mixed separately and evenly, and then extruded and blown using a five-layer co-extrusion device. The film bubble is stable and not prone to wrinkles and folds. The qualified rate of the finished product is high and it is more suitable for actual industrial production. The blown film has good stability, so that the film has the advantages of good blown film processability, high toughness and high strength, can adapt to high-temperature cooking, and is not prone to thermal expansion and bag bursting.

[0023] Optionally, the traction speed is 15-20 m / min and the blowing ratio is 2-3:1.

[0024] By adopting the above technical solution, the traction speed is controlled during inflation, which can prevent defects or ruptures on the bubble surface and reduce the impact on the mechanical strength of the PE film. The inflation ratio can improve the thickness, transparency and strength of the PE film.

[0025] In summary, this application has the following beneficial effects: 1. Since the present application adopts five-layer co-extrusion to prepare the PE film, and all of them are made of a single material, which is easy to recycle, and the inner layer is LDPE, LLDPE and MLLDPE with lower density, the density of the inner layer can be reduced as much as possible, thereby reducing the sealing temperature, improving the heat sealing effect, reducing the damage of the heat seal to the PE film, and improving the barrier properties. Moreover, from the outside to the inside, the addition amount of the barrier masterbatch is arranged in the order of high-low-high-low, which can play a zigzag pulse role and maximize the barrier properties of the PE film.

[0026] 2. In this application, two MLLDPE seat inner layer materials with different densities and melt indexes are preferably used to further reduce the density of the inner layer from the raw material, increase the heat sealing performance, and improve the tear resistance and puncture resistance.

[0027] 3. In the present application, it is preferred to use oxidized cellulose nanofibrils, polyvinyl alcohol and aramid fibers to prepare barrier masterbatch. Oxidized cellulose nanofibrils and polyvinyl alcohol can form a hydrophobic matrix film through multiple hydrogen bonds, and the dispersion formed by aramid fibers can form aerogel on the matrix film through freeze-drying, thereby extending the gas permeation path and improving the barrier capacity to water vapor and oxygen. DETAILED DESCRIPTION

[0028] The following examples further illustrate the present application in detail.

[0029] Preparation Example I-1 of tristearate modified silica: Dry the nano-silica at 60°C for 24h, mix 300mL of anhydrous ethanol and 100mL of deionized water, add 4g of dried nano-silica, and disperse by ultrasound for 2h; take 0.8g of silane coupling agent KH570, stir and hydrolyze with 10mL of anhydrous ethanol and 10mL of acetic acid solution with a pH of 3 (diluted with glacial acetic acid) for 1h, add the hydrolyzate to the nano-silica dispersion after ultrasound, stir in a constant temperature water bath at 75°C for 4h, centrifuge at 8000r / min for 10min, and take the precipitate and vacuum dry it at 80°C for 48h.

[0030] Preparation Example 1-4 of Barrier Masterbatch Preparation Example 1: 35 g of TEMPO-oxidized cellulose nanofibrils were added to deionized water, and ultrasonically dispersed for 2 h at 60 W to prepare a suspension with a concentration of 0.5 wt%. 35 g of polyvinyl alcohol was added to deionized water, stirred at 90 ° C for 1 h, cooled and degassed to prepare a polyvinyl alcohol aqueous solution with a concentration of 3.5 wt%. Aramid fibers were broken into 5 mm fragments, added to ethanol, and ultrasonically removed at 50 W for 30 min. 20 g of the aramid fibers after impurity removal were taken and added to DMSO / H2O (volume ratio of 25:1). , then add 30g potassium hydroxide, mechanically stir at 800r / min for 8h to obtain a dispersion with a concentration of 0.7wt%, add tristearate-modified silica to the dispersion, the mass ratio of aramid fiber to tristearate-modified silica is 1:0.2, tristearate-modified silica is prepared by Preparation Example I-1, TEMPO oxidized cellulose nanofibrils are selected from Zhejiang Jinjiahao green nanoparticles, item number 009, aramid fiber fineness is 400D, and polyvinyl alcohol is PVA1799; The polyvinyl alcohol aqueous solution and the suspension were mixed, stirred at 800 r / min for 3 h at 50 ° C, vacuum degassed, cast into a film, dried at room temperature for 24 h, then dried at 45 ° C for 48 h, and then dried at 60 ° C for 48 h, with a film thickness of 5 μm; The base film was immersed and pulled in the dispersion for 5 times, and then immersed in a 60°C, 50wt% tert-butyl alcohol solution for 3 minutes, the base film was taken out, and washed repeatedly with ultrapure water and anhydrous ethanol for 5 times, and then frozen to -70°C, and then freeze-dried and crushed to obtain an initial powder; The initial powder and No. 1 HDPE were mixed in a mass ratio of 0.06:1, melted, extruded and granulated at 150°C. The density of No. 1 HDPE was 0.969 gg / cm 3 , the melt index is 1.2g / 10min, selected from Dow Chemical of the United States, model AT6900.

[0031] Preparation Example 2: 60 g of TEMPO-oxidized cellulose nanofibrils were added to deionized water, and ultrasonically dispersed for 1 h at 60 W to prepare a suspension with a concentration of 1 wt%. 40 g of polyvinyl alcohol was added to deionized water, stirred at 90 ° C for 1 h, cooled and degassed to prepare a polyvinyl alcohol aqueous solution with a concentration of 4 wt%. Aramid fibers were broken into 3 mm fragments, added to ethanol, and ultrasonically removed at 50 W for 30 min. 20 g of the aramid fibers after impurity removal were taken and added to DMSO / H2O (volume ratio of 25:1), and then added 30g potassium hydroxide, mechanically stirred at 800r / min for 8h to obtain a dispersion with a concentration of 0.5wt%, tristearin modified silica was added to the dispersion, the ratio of tristearin modified silica to the aramid fiber in the dispersion was 0.2:1, tristearin modified silica was prepared by Preparation Example I-1, TEMPO oxidized cellulose nanofibrils were selected from Zhejiang Jinjiahao Green Nanoparticles, item number 009, the aramid fiber fineness was 400D, and the polyvinyl alcohol was PVA1799; The polyvinyl alcohol aqueous solution and the suspension were mixed, stirred at 800 r / min for 3 h at 50 ° C, vacuum degassed, cast into a film, dried at room temperature for 24 h, then dried at 45 ° C for 48 h, and then dried at 60 ° C for 48 h, with a film thickness of 5 μm; The base film was immersed and pulled in the dispersion liquid for 3 times, and then immersed in a tert-butyl alcohol solution with a concentration of 55 wt% at 70° C. for 1 minute, the base film was taken out, and washed repeatedly with ultrapure water and anhydrous ethanol for 3 times, and then frozen to -70° C., and then freeze-dried and crushed to obtain an initial powder; The initial powder and No. 1 HDPE were mixed in a mass ratio of 0.03:1, melted, extruded and granulated at 150°C. The density of No. 1 HDPE was 0.969 gg / cm 3 , the melt index is 1.2g / 10min, selected from Dow Chemical of the United States, model AT6900.

[0032] Preparation Example 3: The difference from Preparation Example 1 is that tristearate-modified silicon dioxide is not added to the dispersion.

[0033] Preparation Example 4: 35 g of TEMPO-oxidized cellulose nanofibrils were added to deionized water, and subjected to ultrasonic dispersion treatment at 60 W for 2 h to prepare a suspension with a concentration of 0.5 wt%. 35 g of polyvinyl alcohol was added to deionized water, stirred at 90 ° C for 1 h, cooled and degassed to prepare a polyvinyl alcohol aqueous solution with a concentration of 3.5 wt%. Aramid fibers were broken into 5 mm fragments, added to ethanol, and ultrasonically removed at 50 W for 30 min. 20 g of the aramid fibers after impurity removal were taken and added to DMSO / H2O (volume ratio of 25:1), and then 30 g of potassium hydroxide was added, and mechanically stirred at 800 r / min for 8 h to prepare a dispersion with a concentration of 0.7 wt%. TEMPO-oxidized cellulose nanofibrils were selected from Zhejiang Jinjiahao Green Nanoparticles, item number 009, the aramid fiber fineness was 400D, and the polyvinyl alcohol was PVA1799. The polyvinyl alcohol aqueous solution and the suspension were mixed, stirred at 800 r / min for 3 h at 50°C, vacuum degassed, cast into a film, dried at room temperature for 24 h, then dried at 45°C for 48 h, and then dried at 60°C for 48 h, with a film thickness of 5 μm, and crushed to obtain an initial powder; The initial powder and No. 1 HDPE were mixed in a mass ratio of 0.06:1, melted, extruded and granulated at 150°C. The density of No. 1 HDPE was 0.969 gg / cm 3 , the melt index is 1.2g / 10min, selected from Dow Chemical of the United States, model AT6900. Example

[0034] Example 1: A low-temperature sealing high temperature-resistant and water-resistant PE film, which includes an inner layer, a sub-inner layer, a middle layer, a sub-outer layer and an outer layer from the inside to the outside, and the thickness ratio of the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer is 2:1:3:1:2. The amount of raw materials used in each layer is shown in Table 1. The melt index of LDPE in the inner layer is 1.9 g / 10 min, and the density is 0.924 g / cm 3 , selected from CNOOC Shell, model 2420, LLDPE selected from Kuwait EQUATE, model 7050, density 0.918g / cm 3 The melt index is 2g / 10min. The MLLDPE includes No. I MLLDPE and No. II MLLDPE with a mass ratio of 1:2. The density of No. I MLLDPE is 0.915g / cm 3 , melt index is 1g / 10min, selected from Japan Ripman, model is SP0820, and the density of II MLLDPE is 0.913g / cm 3 , the melt index is 2g / 10min, selected from Mitsui Metallocene, model is SP1520, the opening agent is oleamide, and the lubricant is ethylene bisoleamide; The HDPE in the secondary inner layer includes No. 1 HDPE and No. 2 HDPE with a mass ratio of 1:1.5. The density of No. 1 HDPE is 0.969 g / cm 3 , the melt index is 1.2g / 10min, selected from Dow Chemical of the United States, model AT6900, the density of No. 2 HDPE is 0.95g / cm3, the melt index is 0.9g / 10min, selected from Yanshan Petrochemical, model 5000S; The HDPE in the middle layer includes No. 1 HDPE and No. 3 HDPE with a mass ratio of 1:1.5. The density of No. 1 HDPE is 0.969g / cm 3 , melt index is 1.2g / 10min, selected from Dow Chemical, USA, HDPE No. 3 density is 0.956g / cm 3 , density is 1g / 10min, selected from Total of South Korea, model is F920A; The HDPE in the secondary outer layer includes No. 1 HDPE and No. 4 HDPE with a mass ratio of 1:1.5. The density of No. 1 HDPE is 0.969 g / cm 3 The melt index is 1.2g / 10min, selected from Dow Chemical, USA, and the loss of No. 4 HDPE is 0.958g / cm 3 , melt index is 0.28g / 10min, selected from DowDuPont of the United States, model is DMDB-6200T; The density of LLDPE in the outer layer is 0.9188g / cm3, the melt index is 1.9gg / 10min, it is selected from Lanzhou Petrochemical, the model is 7042N, and the density of MLLDPE is 0.94g / cm 3 , melt index is 0.9g / 10min, selected from Exxon Chemical 4009MA, HDPE density is 0.961g / cm 3 , melt index is 0.7g / 10min, selected from Exxon Chemical, model is HTA108, antioxidant is antioxidant 1010; The barrier masterbatches in the sub-inner layer, middle layer, sub-outer layer and outer layer are all selected from Dongguan Ruiyi Polymer Materials, model PE9413, and the PPA additives in the five layers are all selected from DuPont Z200.

[0035] The method for preparing the above-mentioned low-temperature sealing high temperature-resistant and water-resistant PE film comprises the following steps: The raw materials in the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are respectively mixed evenly to obtain the inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material; The inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material are added into the hopper of the extruder accordingly, and melted by extrusion. The temperature of each zone of the inner layer extruder is: 150°C in zone 1, 150°C in zone 2, 155°C in zone 3, 160°C in zone 4, 160°C in zone 5, and 155°C in zone 6. The speed of the inner layer main engine is 65r / min. The temperature of each zone of the sub-inner layer extruder is: 155°C in zone 1, 155°C in zone 2, 160°C in zone 3, and 155°C in zone 6. 0℃, 165℃ in zone 4, 165℃ in zone 5, 160℃ in zone 6, the speed of the main machine of the sub-inner layer is 70r / min, the temperature of each zone of the middle layer extruder is: 160℃ in zone 1, 160℃ in zone 2, 165℃ in zone 3, 170℃ in zone 4, 170℃ in zone 5, 165℃ in zone 6, the speed of the main machine of the middle layer is 70r / min, the temperature of the sub-outer layer extruder is: 155℃ in zone 1, 155℃ in zone 2, 160℃ in zone 3, The temperature of the fourth zone is 165℃, the fifth zone is 165℃, and the sixth zone is 160℃. The speed of the outer layer main machine is 70r / min. The temperatures of each zone of the outer layer extruder are: 155℃ in zone 1, 155℃ in zone 2, 160℃ in zone 3, 160℃ in zone 4, 160℃ in zone 5, and 155℃ in zone 6. The speed of the inner layer main machine is 65r / min. Then, the film is blow-molded at an air pressure of 1.5MPa, and the blowing ratio is controlled to be 3:1. The internal cooling air inlet frequency of the rotating air shaft cooler is 20Hz, and the internal cooling exhaust frequency is 25Hz. The molten rubber is pulled upward and quickly kneaded. The pulling speed is 20m / min, and compressed air is rushed into the inflation port of the die head to control the blowing ratio to be 3:1, and the film bubble is pulled up at a uniform speed with a pulling rope; then the film bubble is pulled into the corona machine through the guide roller, and the discharge power of the corona machine is 6A. After that, it passes through the correction clip and enters the winding roller machine to obtain a PE film with a thickness of Wie60μm.

[0036] Table 1 Raw material dosage of low temperature sealing high temperature resistant water barrier PE film in Examples 1-7 Example 2-3: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the raw material amounts of the inner layer, sub-inner layer, middle layer, sub-outer layer and outer layer are as shown in Table 1, and the thickness ratios of the inner layer, sub-inner layer, middle layer, sub-outer layer and outer layer are 2.5:1.5:2.8:1.5:2.5.

[0037] Example 4: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the raw material dosage is as shown in Table 1, and No. II MLLDPE is used in the inner layer instead of No. I MLLDPE.

[0038] Example 5: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the raw material dosage is as shown in Table 1, and No. I MLLDPE is used in the inner layer instead of No. II MLLDPE.

[0039] Example 6: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the raw material dosage is as shown in Table 1, and No. 1 HDPE is used instead of No. 2 HDPE in the sub-inner layer, the middle layer and the sub-outer layer.

[0040] Example 7: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the raw material dosage is as shown in Table 1, and only No. 1 HDPE is added to the sub-inner layer, the middle layer and the sub-outer layer, and No. 2 HDPE is not added.

[0041] Example 8: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the barrier masterbatch in the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are all made from Preparation Example 1.

[0042] Example 9: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the barrier masterbatch in the sub-inner layer, the middle layer, the sub-outer layer and the outer layer is made from Preparation Example 2.

[0043] Example 10: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the barrier masterbatch in the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are all made from Preparation Example 3.

[0044] Example 11: A low-temperature sealing PE film with high temperature resistance and water resistance. The difference from Example 1 is that the barrier masterbatch in the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are all made from Preparation Example 4.

[0045] Comparative Example Comparative Example 1: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the raw material dosage is as shown in Table 2, and MLLDPE is not added to the inner layer.

[0046] Comparative Example 2: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the raw material dosage is as shown in Table 2, and no barrier masterbatch is added to the sub-inner layer, the middle layer and the sub-outer layer.

[0047] Comparative Example 3: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the amount of raw materials used is as shown in Table 2, and the amount of barrier masterbatch added in the sub-inner layer, the middle layer and the sub-outer layer is adjusted to 3 kg.

[0048] Comparative Example 4: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the raw material dosage is as shown in Table 2, and MLLDPE is used in the outer layer instead of HDPE.

[0049] Comparative Example 5: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the raw material dosage is as shown in Table 2, and MLLDPE is not added to the outer layer.

[0050] Comparative Example 6: A low-temperature sealing PE film with high temperature resistance and water resistance, which is different from Example 1 in that the raw material dosage is as shown in Table 2, and MLLDPE and HDPE are not added to the outer layer.

[0051] Table 2 Raw material dosage of low temperature sealing high temperature resistant water barrier PE film in comparative examples 1-6 Performance Testing The PE film was prepared according to the methods in the above examples and comparative examples, and the performance testing was carried out according to the following method. The test results are recorded in Table 3.

[0052] 1. Water vapor transmission rate: According to GB / T26253-2010 "Determination of water vapor transmission rate of plastic film and sheeting by infrared detector method", the test temperature is 38°C, the test humidity is 90% RH, the test flow rate is 20mL / min, and the test area is 50.24cm 2 .

[0053] 2. Oxygen permeability: Tested in accordance with GB / T19789-2022 "Coulometric Test Method for Oxygen Permeability of Films and Sheets", the test temperature is 23SSD, the oxygen partial pressure is 0.1MPa, the test humidity is 0%RH, and the test area is 50.24cm 2 .

[0054] 3. Sealing start temperature and heat sealing strength: The prepared PE film was compounded with a 12μm thick PET film, wherein the inner layer was in contact with the PET film. The starting heat sealing temperature of the composite film was tested according to QB / T 2358-1998 (the temperature when the heat sealing strength reached 10N / 15mm was defined as the starting heat sealing temperature), the heat sealing pressure was 2Bar, the time was 1s, and the heat sealing strength of the film was tested at 100℃.

[0055] 4. Tensile strength: Tested in accordance with GB / T13022-1991 "Test method for tensile properties of plastic films".

[0056] 5. Heat shrinkage resistance: The test is carried out in accordance with GB / T12027-2004 "Test method for dimensional change rate of plastic film and sheeting when heated", and the test temperature is 130℃.

[0057] Table 3 Performance test of low temperature sealing high temperature resistance and water barrier PE film It can be seen from the data in Examples 1-3 and Table 3 that the PE film has a low sealing temperature, high heat sealing strength, low water vapor and oxygen permeability, good water and oxygen barrier effects, and strong heat resistance.

[0058] Compared with Example 1, Example 4 does not add No. I MLLDPE in the inner layer, and No. II MLLDPE is used instead of No. I MLLDPE. Compared with Example 1, No. I MLLDPE is used instead of No. II MLLDPE in Example 5. The data in Table 3 show that the water-barrier and oxygen-barrier effects of the PE films prepared in Examples 4 and 5 are not as good as those in Example 1, and the tensile strength is reduced, the sealing temperature is increased, and the heat-sealing strength is reduced.

[0059] Compared with Example 1, in Example 6, No. 1 HDPE is used instead of No. 2 HDPE in the sub-inner layer, the middle layer and the sub-outer layer. Compared with Example 1, No. 2 HDPE is not added in Example 7. It can be seen that the PE films prepared in Examples 6 and 7 have reduced barrier properties to water vapor and oxygen, and the barrier property is more significantly reduced in Example 7. At the same time, the thermal shrinkage rate is also increased, and the heat resistance is weakened.

[0060] Compared with Example 1, Example 8 and Example 9 use the barrier masterbatch prepared by Preparation Example 1 and Preparation Example 2. Compared with Example 1, the PE films prepared in Example 8 and Example 9 have improved water barrier and oxygen barrier properties to water vapor and oxygen, improved tensile strength, reduced thermal shrinkage, and increased heat resistance.

[0061] In Example 10, the barrier masterbatch prepared in Preparation Example 3 was used. Compared with Preparation Example 1, tristearate-modified silica was not added. In Example 11, the barrier masterbatch prepared in Preparation Example 4 was used, in which the aramid fiber dispersion was not impregnated. In Example 10, it was shown that the barrier ability of the PE film to water vapor and oxygen decreased, and the tensile strength was weakened. In Example 11, the barrier ability decreased more significantly.

[0062] Compared with Example 1, Comparative Example 1 does not add MLLDPE in the inner layer. Table 3 shows that the PE film prepared in Comparative Example 1 has a decreased barrier capacity to water vapor and oxygen, a decreased sealing temperature, a decreased heat sealing strength, and weakened tensile strength and heat resistance.

[0063] In Comparative Example 2, barrier masterbatch was not added to the sub-inner layer, the middle layer and the sub-outer layer, but only to the outer layer. In Comparative Example 3, the amount of barrier masterbatch in the sub-outer layer, the sub-inner layer, the middle layer and the outer layer was 3 kg, with a unified flux. Compared with Example 1, the barrier property in Comparative Example 3 was higher than that in Comparative Example 2, and the barrier property in Comparative Example 2 was the worst. It can be seen that the amount of barrier masterbatch is arranged in the order of high-low-high-low from the outer layer to the sub-inner layer, which can significantly improve the water and oxygen barrier capabilities of the PE film.

[0064] Compared with Example 1, Comparative Example 4 uses MLLDPE instead of HDPE in the outer layer, and compared with Example 1, Comparative Example 5 does not add MLLDPE in the outer layer, and compared with Example 1, Comparative Example 6 does not add MLLDPE and HDPE in the outer layer. It can be seen from the data in Table 3 that the various properties of the PE film in Comparative Example 6 are the worst, and Comparative Example 4 is the best. The combination of MLLDPE and HDPE can improve the barrier properties of the PE film.

[0065] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low temperature sealing high temperature resistance and water barrier PE film, characterized in that: From the inside to the outside, it includes the following five layers: inner layer, sub-inner layer, middle layer, sub-outer layer and outer layer; The inner layer comprises the following raw materials in parts by weight: 8-12 parts of LDPE, 25-35 parts of LLDPE, 55-65 parts of MLLDPE, 0.6-1 parts of PPA additive, 1.2-2 parts of lubricant, and 5-6 parts of opening agent; The secondary inner layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 1-2 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additive; The middle layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 2.5-3.5 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additive; The secondary outer layer comprises the following raw materials in parts by weight: 90-100 parts of HDPE, 2-3 parts of barrier masterbatch, and 0.2-0.6 parts of PPA additive; The outer layer comprises the following raw materials in parts by weight: 35-45 parts of LLDPE, 25-35 parts of MLLDPE, 25-35 parts of HDPE, 3.5-4 parts of barrier masterbatch, 0.2-0.6 parts of PPA additive, and 0.2-0.6 parts of antioxidant.

2. The low temperature sealing high temperature resistance and water barrier PE film according to claim 1, characterized in that: The inner layer includes MLLDPE with a mass ratio of 1:1.5-2 and a density of 0.915 g / cm 3 , No. 1 MLLDPE with a melt index of 1 g / 10 min and a density of 0.913 g / cm 3 , No. II MLLDPE with a melt index of 2g / 10min.

3. The low temperature sealing high temperature resistance and water barrier PE film according to claim 1, characterized in that: The HDPE in the secondary inner layer has a mass ratio of 1:1.5-2 and a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.950g / cm 3 , No. 2 HDPE with a melt index of 0.9g / 10min; The HDPE in the middle layer has a mass ratio of 1:1.5-2 and a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.956g / cm 3 , No. 3 HDPE with a density of 1g / 10min; The HDPE in the secondary outer layer has a mass ratio of 1:1.5-2 and a density of 0.969 g / cm 3 , No. 1 HDPE with a melt index of 1.2g / 10min and a density of 0.958g / cm 3 , No. 4 HDPE with a density of 0.28g / 10min.

4. The low temperature sealing high temperature resistance and water barrier PE film according to claim 3, characterized in that: The density of LLDPE in the outer layer is 0.9188 g / cm 3 , melt index is 1.9g / 10min, density of MLLDPE is 0.94g / cm 3 , melt index is 0.9g / 10min, density of HDPE is 0.961g / cm 3 , the melt index is 0.7g / 10min.

5. The low temperature sealing high temperature resistance and water barrier PE film according to claim 1, characterized in that: The density of LDPE in the inner layer is 0.924 g / cm 3 , melt index is 1.9g / 10min, density of LLDPE is 0.918g / cm 3 , the melt index is 2g / 10min.

6. The low temperature sealing high temperature resistance and water barrier PE film according to claim 3, characterized in that: The preparation method of the barrier masterbatch is as follows: The oxidized nanocellulose fibrils were subjected to ultrasonic dispersion treatment with deionized water for 1-2 hours to prepare a suspension with a concentration of 0.5-1wt%, polyvinyl alcohol was dissolved in deionized water to prepare a polyvinyl alcohol aqueous solution with a concentration of 3.5-4wt%, and aramid fibers were broken into 3-5mm fragments, added to ethanol, ultrasonically removed impurities, and then dissolved to prepare a dispersion with a concentration of 0.5-0.7wt%; The polyvinyl alcohol aqueous solution and the suspension are mixed, stirred evenly, degassed, cast, and dried to obtain a matrix film, wherein the mass ratio of the oxidized nanocellulose fibrils to the polyvinyl alcohol is 1-1.5:1; The base film is immersed and pulled in the dispersion for 3-5 times, and then immersed in a tert-butyl alcohol solution with a concentration of 50-55 wt% and a temperature of 60-70° C. for 1-3 minutes, taken out and repeatedly washed with ultrapure water and anhydrous ethanol, freeze-dried, and crushed to obtain an initial powder; The initial powder and No. 1 HDPE were mixed, melted and granulated in a mass ratio of 0.03-0.06:

1.

7. The low temperature sealing high temperature resistance and water barrier PE film according to claim 6, characterized in that: The dispersion is further added with tristearic acid glyceryl modified silicon dioxide, and the mass ratio of tristearic acid glyceryl modified silicon dioxide to the aramid fiber in the dispersion is 0.1-0.2:

1.

8. The low temperature sealing high temperature resistance and water barrier PE film according to claim 1, characterized in that: The thickness ratio of the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer is 2-2.5:1-1.5:2.8-3:1-1.5:2-2.

5.

9. The method for preparing the low temperature sealing high temperature resistant and water resistant PE film according to any one of claims 1 to 8, characterized in that: The following steps are involved: The raw materials in the inner layer, the sub-inner layer, the middle layer, the sub-outer layer and the outer layer are respectively mixed evenly to obtain the inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material; The inner layer material, the sub-outer layer material, the middle layer material, the sub-outer layer material and the outer layer material are added into the hopper of the extruder respectively, and the PE film is obtained through extrusion melting, casting, film drawing, blowing, pulling and winding.

10. The method for preparing the low-temperature sealing high temperature-resistant and water-resistant PE film according to claim 8, characterized in that: The pulling speed is 15-20 m / min, and the blowing ratio is 2-3:1.

Citation Information

Patent Citations

  • High-resistance polymer coating fluid

    CN102382525A

  • Barrier master batch for preparing polyethylene film and preparation method of barrier master batch

    CN113754949A

  • High-barrier single PE recyclable material packaging film and production process thereof

    CN115447241A

  • Preparation method and application of photo-thermal antibacterial composite film

    CN117887115A

  • High-barrier polyolefin composite film and preparation method thereof

    CN118046649A