Modified basalt fiber-glass fiber composite material and biological induction material of artificial shellfish algal reef as well as preparation method and application of modified basalt fiber-glass fiber composite material and biological induction material

By modifying the combination of basalt fiber-glass fiber composite materials and multiple raw materials, the adhesion difficulties caused by the singleness of artificial shell algae reefs are solved, and the adhesion rate of oyster larvae and large algae and the stability of ecosystems are improved. .

CN119038890APending Publication Date: 2024-11-29OCEAN UNIV OF CHINA
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411159442.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing artificial shell algae reef has a single material, which leads to low metamorphism of oyster larvae, difficulty and slow attachment of oyster larvae and large algae spores, affecting the effect of ecosystem construction.

Method used

Modified basalt fiber-glass fiber composite material is used to modify basalt fibers through nanosilicon dioxide and nanoceramic particles, and coupled with glass fibers to form a material with rich surfactant groups and three-dimensional grid structure, combined with steel slag powder , sulfate cement, fly ash and modified straw to enhance the corrosion resistance and adhesion of the material.

Benefits of technology

It significantly improves the adhesion rate and adhesion amount of oyster larvae and large algae, improves the compressive strength, porosity and wear rate of artificial shellfish reefs, extends the service life, and improves the ecological habitat effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006015460000151
    Figure BDA0005006015460000151
  • Figure BDA0005006015460000152
    Figure BDA0005006015460000152
  • Figure BDA0005006015460000161
    Figure BDA0005006015460000161
Patent Text Reader

Abstract

The invention discloses a modified basalt fiber-glass fiber composite material of an artificial shellfish algal reef, a biological induction material as well as a preparation method and application of the biological induction material, and belongs to the technical field of material preparation. The preparation method of the modified basalt fiber-glass fiber composite material comprises the following steps: modifying basalt fibers with nano silicon dioxide and nano ceramsite to obtain modified basalt fibers, and coupling the modified basalt fibers and glass fibers to obtain the modified basalt fiber-glass fiber composite material. According to the preparation method, the specific surface area of the basalt fiber can be increased, the surface has rich surface active groups, the washing resistance, durability and corrosion resistance of the material are improved, the porosity is high, more micropores and channels can be formed, attachment of oyster larvae and macroalgae spores is promoted, and the service life of the material is prolonged. The construction of the shellfish-algal reef composite habitat is promoted, and the construction effect of the shellfish-algal reef composite habitat is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a modified basalt fiber-glass fiber composite material and a biological induction material for an artificial shellfish and algae reef, and a preparation method and application thereof. Background Art

[0002] Artificial shellfish and algae reefs refer to artificial facilities composed of one or more natural or artificial structures and purposefully placed in the sea to promote the attachment of large seaweed and oysters, and to improve the ecological environment of the waters, increase fishery resources, and promote social and economic development based on natural reproduction, growth and expansion. The construction of artificial shellfish and algae reefs is one of the marine fishery ecological projects that have emerged in recent years and is an important part of marine ranches. The creation of artificial shellfish and algae reef habitats promotes the recovery of marine biological resources including large algae and shellfish and the improvement of the marine ecological environment through the deployment of artificial reefs, reproduction and release, etc. It has become an important consensus of coastal countries to promote the sustainable development of offshore fisheries, and has achieved good results through years of practice.

[0003] At present, the materials used to build artificial shellfish and algae reefs are relatively simple, and the common reef-building materials are mainly reinforced concrete, stone, steel, wood and shells. Since reinforced concrete has high tensile strength and compressive strength, it is the most widely used material in the construction of artificial shellfish and algae reefs. However, in the process of reef production, in addition to the main materials of steel bars and cement, only necessary additives are added, and the selection of reef materials is highly homogenized. Moreover, after being released into natural sea areas, there are also problems such as low metamorphosis rate of oyster larvae, difficulty and slow attachment of oyster larvae and large algae spores, which directly affect the construction effect of the algae reef composite ecosystem. Therefore, providing a material that adds a variety of beneficial materials, has a wide source and little impact on the environment, is conducive to inducing the metamorphosis of oyster larvae, and promotes the attachment of oyster larvae and large algae spores, is of great significance to improving the effect of creating a composite habitat for shellfish and algae reefs. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a method for preparing a modified basalt fiber-glass fiber composite material, and the prepared composite material can increase the attachment rate of large algae and oyster larvae.

[0005] Another object of the present invention is to provide a modified basalt fiber-glass fiber composite material prepared by the modified basalt fiber-glass fiber composite material preparation method.

[0006] Another object of the present invention is to provide an artificial shellfish and algae reef biological induction material.

[0007] Another object of the present invention is to provide a method for preparing the artificial shellfish and algae reef biological induction material.

[0008] Another object of the present invention is to provide a method for preparing the modified basalt fiber-glass fiber composite material or the modified basalt fiber-glass fiber composite material or the artificial shellfish and algae reef biological induction material or the method for preparing the artificial shellfish and algae reef biological induction material and use them in preparing artificial reefs and / or constructing artificial shellfish and algae reef habitats.

[0009] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0010] The present invention provides a method for preparing a modified basalt fiber-glass fiber composite material, comprising the following steps:

[0011] Nano silicon dioxide and nano ceramsite are dispersed in an alcohol solution to obtain a mixed dispersion; basalt fiber is immersed in a strong alkaline solution to obtain treated basalt fiber; the treated basalt fiber and vinyl tri(β-methoxyethoxy)silane are added to the mixed dispersion to react to obtain modified basalt fiber; the modified basalt fiber and glass fiber are coupled to obtain the modified basalt fiber-glass fiber composite material.

[0012] Preferably, the mass volume ratio of the nano-silicon dioxide, nano-ceramsite and alcohol solution is 1g: 0.8-1.2g: 110-130mL.

[0013] Preferably, the immersion temperature of the basalt fiber in the strong alkaline solution is 55-70° C., and the immersion time is 9-11 hours.

[0014] Preferably, the reaction temperature is 85-90° C., and the reaction time is 4-6 hours.

[0015] Preferably, the coupling method comprises: adding the modified basalt fiber and glass fiber to a coupling agent, and reacting at 165-175° C. for 2-3 hours.

[0016] The present invention also provides a modified basalt fiber-glass fiber composite material prepared by any one of the preparation methods described above.

[0017] The present invention also provides an artificial shellfish and algae reef biological induction material, comprising the following components by weight: 45-55 parts of steel slag powder, 28-42 parts of sulfate cement, 30-45 parts of fly ash, 15-30 parts of cattle bone powder, 16-20 parts of the above-mentioned modified basalt fiber-glass fiber composite material and 12-18 parts of modified straw;

[0018] The modified straw is prepared by enzymatic hydrolysis and oxidation of the straw.

[0019] Preferably, the enzymatic enzymes include cellulase and hemicellulase.

[0020] Preferably, the oxidizing oxidant comprises potassium permanganate and / or hydrogen peroxide.

[0021] The present invention also provides a method for preparing the artificial shellfish and algae reef biological induction material described in any one of the above items, comprising the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them, adding water and stirring to obtain the artificial shellfish and algae reef biological induction material.

[0022] The present invention also provides a method for preparing the modified basalt fiber-glass fiber composite material described in any one of the above or the use of the modified basalt fiber-glass fiber composite material or the artificial shellfish and algae reef biological induction material described in any one of the above or the method for preparing the artificial shellfish and algae reef biological induction material in preparing artificial reefs and / or constructing artificial shellfish and algae reef habitats.

[0023] Beneficial effects of the present invention:

[0024] The present invention obtains modified basalt fiber by modifying basalt fiber with nano-silicon dioxide and nano-ceramsite, and obtains modified basalt fiber-glass fiber composite material by coupling modified basalt fiber and glass fiber. The preparation method of the present invention can increase the specific surface area of ​​basalt fiber, so that the surface has abundant surface active groups, thereby greatly promoting the attachment and growth of large algae; the modified basalt fiber is coupled with glass fiber to form a three-dimensional grid structure, improve the scour resistance, durability and corrosion resistance of the material, have a higher porosity, and are conducive to forming more micropores and channels, thereby further promoting the attachment of oyster larvae and large algae spores.

[0025] The present invention selects beneficial ingredients such as steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite materials and modified straw as construction materials for artificial shellfish and algae reefs. The raw materials have a wide source and have little impact on the environment. Several raw materials have a composite reinforcement effect. Through multiple mechanisms such as physical reinforcement and chemical stabilization, the surface area of ​​the artificial shellfish and algae reef is increased, the surface roughness of the reef is increased, the stability of the reef structure is improved, and the problem of poor attachment effect of large algae and oyster larvae is solved. Compared with the control group in which the modified basalt fiber-glass fiber composite material or the modified straw was changed, the compressive strength of the artificial shellfish and algae reef biological induction material of the present invention was increased by 8.42%-31.53%, the porosity was increased by 46.73%-97.62%, the abrasion rate was reduced by 14.29%-56.76%, the oyster larvae attachment rate was increased by 20.18%-53.05%, the oyster larvae attachment amount was increased by 28.35%-138.35%, and the algae attachment amount was increased by 47.04%-108.07%.

[0026] The present invention improves the efficiency of inducing metamorphosis of oyster larvae through scientific proportioning and process treatment, promotes the attachment of oyster larvae and large algae spores, promotes the creation of a shellfish-algae reef composite habitat, and improves the ecological effect of the shellfish-algae reef composite habitat. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a modified basalt fiber-glass fiber composite material, comprising the following steps:

[0028] Nano silicon dioxide and nano ceramsite are dispersed in an alcohol solution to obtain a mixed dispersion; basalt fiber is immersed in a strong alkaline solution to obtain treated basalt fiber; the treated basalt fiber and vinyl tri(β-methoxyethoxy)silane are added to the mixed dispersion to react to obtain modified basalt fiber; the modified basalt fiber and glass fiber are coupled to obtain the modified basalt fiber-glass fiber composite material.

[0029] In the present invention, there is no special limitation on the sources of the nano-silicon dioxide, nano-ceramsite, basalt fiber and glass fiber, and they can be purchased through conventional commercial channels or prepared by conventional methods. Nano-ceramsite is a small particle formed by firing an inorganic material at a high temperature, and its particle size is in the nanometer scale, usually less than 100 nanometers, and its main components include aluminum oxide and silicon dioxide. As an optional embodiment, the particle size of the nano-silicon dioxide is preferably 80 to 100 nm, and more preferably 90 nm; the particle size of the nano-ceramsite is preferably 90 to 100 nm, and more preferably 95 nm; the length of the basalt fiber is preferably 8 to 12 mm, and more preferably 10 mm; the length of the glass fiber is preferably 6 to 25 mm, and more preferably 10 to 18 mm.

[0030] In the present invention, as an embodiment, the alcohol solution is preferably one or more of ethanol solution, methanol solution or isopropanol solution; preferably, the alcohol solution is ethanol solution. As an embodiment, the concentration of the alcohol solution is preferably a high concentration. As an optional embodiment, when the alcohol solution is an ethanol solution, the mass concentration of the ethanol solution is preferably 80% to 90%, and more preferably 85%. As an embodiment, when the alcohol solution is an ethanol solution, the mass volume ratio of the nano-silicon dioxide, nano-ceramic particles and the alcohol solution is preferably 1g: 0.8 to 1.2g: 110 to 130mL, and more preferably 1g: 1g: 120mL. When the alcohol solution is a methanol solution or an isopropanol solution, the mass volume ratio of the nano-silicon dioxide, nano-ceramic particles and the alcohol solution can be determined according to the density, solubility and compatibility of the solvent with the nano-ceramic particles.

[0031] In the present invention, as an embodiment, the strong alkali solution includes any one of potassium hydroxide solution, sodium hydroxide solution, calcium hydroxide solution, etc.; preferably, the strong alkali solution is sodium hydroxide solution. As an optional embodiment, the mass concentration of the sodium hydroxide solution is preferably 50% to 60%, and more preferably 55%; as another optional embodiment, when the strong alkali solution is a strong alkali solution other than sodium hydroxide solution, its mass concentration can be converted by the concentration of OH- ions produced by them in water. As an optional embodiment, the mass volume ratio of the basalt fiber and the strong alkali solution is preferably 1g: 400 to 450mL, and more preferably 1g: 420mL. The basalt fiber is soaked in the strong alkali solution, and the soaking temperature is preferably 55 to 70°C, and more preferably 62°C; the soaking time is preferably 9 to 11h, and more preferably 10h. As an embodiment, after the soaking is completed, it can also include filtering, washing and other steps. The filtering and washing methods and times can be conventionally selected according to actual needs to remove the residual strong alkali solution and obtain the treated basalt fiber.

[0032] In the present invention, as an embodiment, the mass volume ratio of the treated basalt fiber, vinyl tri(β-methoxyethoxy)silane and the mixed dispersion is preferably 1g: 5-6g: 220-260mL, and more preferably 1g: 5.5g: 240mL. As an embodiment, the treated basalt fiber and vinyl tri(β-methoxyethoxy)silane are added to the mixed dispersion for reaction, and the reaction temperature is preferably 85-90°C, and more preferably 88°C; the reaction time is preferably 4-6h, and more preferably 5h. As an embodiment, after the reaction is completed, the steps of filtering, washing, drying, etc. can also be included. The methods and times of filtering, washing and drying can be conventionally selected according to actual needs to remove the residual vinyl tri(β-methoxyethoxy)silane and the mixed dispersion to obtain modified basalt fiber.

[0033] In the present invention, vinyl tri(β-methoxyethoxy) silane can form a covalent bond with the substrate surface through its vinyl group, and its methoxyethoxy part can be hydrolyzed to form a silanol group, which further reacts with the fiber surface, which increases the types and number of functional groups on the fiber surface. Nano silicon dioxide and nano ceramsite have a high surface area and abundant surface hydroxyl groups. When combined with the fiber surface, the functional groups on the surface can be further increased by hydrogen bonds or chemical bonds. After the present invention uses vinyl tri(β-methoxyethoxy) silane as a modifier to react with the treated basalt fiber, nano silicon dioxide in the mixed dispersion, and nano ceramsite, it can improve the durability of the basalt fiber, improve its service life and performance, and it also has water resistance and corrosion resistance. Compared with other commonly used modifiers that can only be modified, vinyl tri(β-methoxyethoxy) silane has multiple functions and can significantly improve the durability, water resistance and corrosion resistance of basalt fiber.

[0034] In the present invention, the modified basalt fiber and the glass fiber are coupled, as an embodiment, the coupling method includes adding the modified basalt fiber and the glass fiber to a coupling agent for reaction. As an optional embodiment, the coupling agent is preferably a silane coupling agent; the silane coupling agent includes any one of γ-methacryloxypropyltrimethoxysilane (KH-570 silane coupling agent), γ-methacryloxypropyltriethoxysilane (A-174), vinyltrimethoxysilane (VTMS), vinyltriethoxysilane (VTES), γ-glycidyloxypropyltrimethoxysilane (GPTMS) and γ-aminopropyltriethoxysilane (APTES), preferably KH-570 silane coupling agent. As an optional embodiment, when the coupling agent is KH-570 silane coupling agent, the mass ratio of the modified basalt fiber, glass fiber and coupling agent is preferably 1: 0.4-0.6: 16-20, and more preferably 1: 0.5: 17; as another optional embodiment, when the coupling agent is other silane coupling agents, the mass ratio of the modified basalt fiber, glass fiber and coupling agent can be converted according to the molecular weight of the coupling agent. The reaction temperature is preferably 165-175°C, and more preferably 168°C; the reaction time is preferably 2-3h, and more preferably 2.5h. As an implementable embodiment, after the reaction is completed, the steps of filtering and drying can also be included. The method and number of filtering and drying can be conventionally selected according to actual needs to remove the residual glass fiber and coupling agent to obtain a modified basalt fiber-glass fiber composite material.

[0035] The present invention also provides a modified basalt fiber-glass fiber composite material prepared by any one of the preparation methods described above.

[0036] The present invention utilizes nano-silicon dioxide and nano-ceramsite to modify basalt fiber, removes impurities and pollutants on the fiber surface by alkali washing, further increases the hydroxyl group (-OH) on the fiber surface, and increases the surface active site (-OH); surface modification by nano-silicon dioxide can effectively improve its structural stability; nano-ceramsite combines with the fiber surface by physical adsorption and surface chemical reaction, and increases the fiber surface area and pore structure. The three work together to increase the specific surface area of ​​basalt fiber and thus provide more attachment points for the growth of large algae and oyster larvae; modification by nano-ceramsite and nano-silicon dioxide can also make basalt fiber have excellent wear resistance and corrosion resistance, thereby improving the seawater corrosion resistance and scouring resistance of artificial shellfish reefs; basalt fiber modified by nano-silicon dioxide and nano-ceramsite has abundant surface active groups, so that the prepared artificial shellfish reef can react with nutrients and large algae cells in seawater, thereby forming a strong chemical bond, thereby greatly promoting the attachment and growth of large algae. The present invention further selects a composite material prepared by compounding glass fiber and basalt fiber. The two are compounded in the artificial shellfish reef to form a three-dimensional grid structure, which greatly improves the scour resistance and durability of the reef. The glass fiber and modified basalt fiber have excellent tolerance to acids, alkalis and salt substances. After processing and compounding, the corrosion resistance of the reef can be further improved. After the glass fiber and the modified basalt fiber are compounded, the porosity of the reef material is also improved, which is conducive to the formation of more micropores and channels, thereby further promoting the attachment and growth of large algae.

[0037] The present invention also provides an artificial shellfish and algae reef biological induction material, which preferably comprises the following components in parts by mass: 45-55 parts of steel slag powder, 28-42 parts of sulfate cement, 30-45 parts of fly ash, 15-30 parts of cattle bone powder, 16-20 parts of the above-mentioned modified basalt fiber-glass fiber composite material and 12-18 parts of modified straw; the steel slag powder is more preferably 50 parts, and / or the sulfate cement is more preferably 30 parts; and / or the fly ash is more preferably 43 parts; and / or the cattle bone powder is more preferably 30 parts; and / or the modified basalt fiber-glass fiber composite material is more preferably 18 parts; and / or the modified straw is more preferably 16 parts;

[0038] The modified straw is preferably prepared by enzymatic hydrolysis and oxidation of straw.

[0039] In the present invention, there is no special limitation on the sources of the steel slag powder, sulfate cement, fly ash and cattle bone powder, and they can be purchased through conventional commercial channels or prepared by conventional methods. As an implementation method, the particle size of the steel slag powder is preferably 8 to 12 mm, more preferably 10 mm; the particle size of the fly ash is preferably 150 to 180 mesh, more preferably 160 mesh; the particle size of the cattle bone powder is preferably 5 to 10 mm, more preferably 8 mm.

[0040] In the present invention, the modified straw is prepared by enzymatic hydrolysis and oxidation of the straw. As an implementable embodiment, the preparation method of the modified straw comprises the following steps: crushing the straw, adding it to water, adjusting the pH, adding an enzyme, soaking, and obtaining primary modified straw powder; adding the primary modified straw powder and an oxidant to water for reaction to obtain the modified straw. In the present invention, there is no special limitation on the type and source of the straw, and conventional crop straws can be selected, including but not limited to one or more of corn straw, wheat straw, rice straw or sorghum straw. As an implementable embodiment, the particle size of the crushed straw is preferably 180 to 220 meshes, and more preferably 220 meshes. After the straw is crushed, straw powder is obtained, and the straw powder is added to water. The mass volume ratio of the straw powder to water is preferably 1g: 180 to 220mL, and more preferably 1g: 200mL. The enzyme is preferably a composite enzyme; the composite enzyme preferably includes a composite enzyme of cellulase and hemicellulase; the cellulase activity is preferably 340-720U / g, more preferably 470-590U / g; the hemicellulase activity is preferably 420-960U / g, more preferably 620-840U / g. The mass ratio of cellulase and hemicellulase in the composite enzyme is preferably 1:0.7-0.9, more preferably 1:0.8. As an embodiment, the mass ratio of straw powder and enzyme is preferably 1:0.013-0.018, more preferably 1:0.016. The pH can be specifically selected according to the type of enzyme added. As an embodiment, when the enzyme includes a composite enzyme of cellulase and hemicellulase, the pH is preferably 5.2-5.7, more preferably 5.5. As an embodiment, the soaking temperature is preferably 52-55°C, more preferably 54°C; the soaking time is preferably 5-8h, more preferably 6h. As an implementable method, after the soaking is completed, filtering and other steps may be further included. The filtering method and number of times may be conventionally selected according to actual needs to obtain primary modified straw powder.

[0041] In the present invention, the primary modified straw powder and the oxidant are added to water for reaction; the oxidant can be conventionally selected according to actual needs, such as potassium permanganate and / or hydrogen peroxide; preferably potassium permanganate. As an implementable embodiment, when the oxidant is potassium permanganate, the mass ratio of the primary modified straw powder and the oxidant is preferably 1:4-6, and more preferably 1:5; as another implementable embodiment, when the oxidant is hydrogen peroxide, the amount of hydrogen peroxide can be determined by conversion according to the stoichiometric relationship of the specific reaction, the reaction conditions and the required degree of oxidation. The present invention does not specifically limit the amount of water, which can be conventionally selected according to actual needs. As an implementable embodiment, the temperature of the reaction is preferably 40-45°C, and more preferably 42°C; the reaction time is preferably 2-3h, and more preferably 2.5h. As an implementable embodiment, after the reaction is completed, the steps of filtration, water washing, drying, etc. can also be included, and the methods and times of filtration, water washing and drying can be conventionally selected according to actual needs to remove the residual oxidant and obtain modified straw.

[0042] The present invention utilizes enzymes to hydrolyze straw, and the enzymatic hydrolysis increases the porosity and surface roughness of the straw by changing the microstructure of the straw, thereby improving the adhesion ability of the artificial algae reef to large algae; further, the primary modified straw is oxidized with an oxidant, and the hydrocarbons on the surface of the primary modified straw can be oxidized into active functional groups such as carboxyl and carbonyl, which can not only promote the reaction with large algae cells and promote the adhesion ability of large algae, but also further enhance the adhesion between the modified straw and other materials in the reef body, thereby improving the strength and scour resistance of the artificial shellfish reef.

[0043] Compared with the prior art, the artificial shellfish reef biological induction material provided by the present invention has steel slag as the main component, which has super corrosion resistance, and it can also promote the attachment of large algae by releasing iron ions. Further, the present invention also adds a specific modified basalt fiber-glass fiber composite material, and the composite of the two fibers forms a three-dimensional grid structure in the artificial shellfish reef, which greatly improves the stability and service life of the reef, and the material obtained by the composite of the modified basalt fiber and the glass fiber also has excellent corrosion resistance, which can also improve the porosity of the reef material, change the reef microstructure, and promote the attachment of large algae and oyster larvae. In the present invention, the basalt fiber is modified by nano-silicon dioxide and nano-ceramsite, and the modified basalt fiber has a large specific surface area and rich surface active groups, thereby improving the attachment and growth ability of large algae and oyster larvae, and the nano-silicon dioxide and nano-ceramsite are attached to the basalt fiber, which further improves the wear resistance and corrosion resistance of the basalt fiber, thereby further improving the seawater corrosion resistance and scouring resistance of the artificial shellfish reef. The addition of fly ash and cow bone meal further improved the performance of the modified basalt fiber-glass fiber composite material. The three materials, through synergistic action, greatly improved the stability of the three-dimensional grid structure, effectively improved the strength and durability of artificial shellfish reefs, and reduced the corrosiveness and scouring of artificial shellfish reefs by the marine environment. In addition, the special structure of fly ash can also absorb ions in seawater to improve the corrosion resistance of artificial shellfish reefs; cow bone meal contains a large amount of organic calcium, which can significantly increase the attachment rate of oyster larvae. At the same time, organic calcium is conducive to the formation and development of microbial membranes. The compounds released by microorganisms on the biofilm are conducive to accelerating the attachment of oyster larvae. The modified straw has an excellent specific surface area and a large number of active groups. It increases the specific surface area of ​​artificial shellfish reefs and increases the attachment ability of large algae and oyster larvae. It can also improve the strength and scouring resistance of artificial shellfish reefs by improving the adhesion with other materials.

[0044] The present invention selects steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw as the basic materials of the shellfish reef, and the raw materials play a composite strengthening effect. Through multiple mechanisms such as physical reinforcement and chemical stabilization, the surface area of ​​the artificial shellfish reef is increased, the surface roughness of the reef is increased, the stability of the reef structure is improved, and the problem of poor attachment effect of large algae and oyster larvae is solved.

[0045] The present invention also provides a method for preparing the artificial shellfish and algae reef biological induction material described in any one of the above items, comprising the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them, adding water and stirring to obtain the artificial shellfish and algae reef biological induction material.

[0046] In the present invention, there is no special limitation on the amount of water, which can be selected and determined according to the actual stirring conditions. As an implementation method, the amount of water can be determined according to the amount of sulfate cement, and the mass ratio of sulfate cement to water is preferably 1:0.4-0.5, and more preferably 1:0.45. The stirring method can be conventionally selected according to actual needs, including manual stirring or mechanical stirring.

[0047] The present invention also provides a method for preparing the modified basalt fiber-glass fiber composite material described in any one of the above or the use of the modified basalt fiber-glass fiber composite material or the artificial shellfish and algae reef biological induction material described in any one of the above or the method for preparing the artificial shellfish and algae reef biological induction material in preparing artificial reefs and / or constructing artificial shellfish and algae reef habitats.

[0048] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0049] In the following embodiments, unless otherwise specified, all of them are conventional methods.

[0050] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0051] In the following examples, nano-silicon dioxide was ordered from Bohuasi Nano-Tech (Ningbo) Co., Ltd., nano-ceramsite was ordered from Jingdezhen Better New Materials Co., Ltd., basalt fiber was purchased from Weifang Zhongchuang Innovation Materials Technology Co., Ltd., and glass fiber was purchased from Jining Hongjun Glass Fiber Co., Ltd.

[0052] Example 1

[0053] This embodiment provides a method for preparing a modified basalt fiber-glass fiber composite material, and the steps are as follows:

[0054] Nano-silicon dioxide and nano-ceramsite are dispersed in an ethanol aqueous solution with a mass concentration of 90% to obtain a mixed dispersion; wherein the mass volume ratio of nano-silicon dioxide, nano-ceramsite and ethanol aqueous solution is 1g:0.8g:110mL, the particle size of nano-silicon dioxide is 80nm, and the particle size of nano-ceramsite is 100nm. Basalt fiber with a length of 12mm is soaked in a sodium hydroxide solution with a mass concentration of 50% at 70°C for 9h, filtered, washed with water, and treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber and sodium hydroxide solution is 1g:400mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the mixed dispersion, reacted at 85°C for 4h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and mixed dispersion is 1g:6g:260mL. The modified basalt fiber and the glass fiber with a length of 14 mm were added to the KH-570 silane coupling agent, reacted at 165° C. for 2 h, filtered, and dried to obtain a modified basalt fiber-glass fiber composite material; wherein the mass ratio of the modified basalt fiber, the glass fiber, and the KH-570 silane coupling agent was 1:0.6:20.

[0055] Example 2

[0056] This embodiment provides a method for preparing a modified basalt fiber-glass fiber composite material, and the steps are as follows:

[0057] Nano-silicon dioxide and nano-ceramsite are dispersed in an ethanol aqueous solution with a mass concentration of 80% to obtain a mixed dispersion; wherein the mass volume ratio of nano-silicon dioxide, nano-ceramsite and ethanol aqueous solution is 1g:1.2g:130mL, the particle size of nano-silicon dioxide is 100nm, and the particle size of nano-ceramsite is 90nm. Basalt fiber with a length of 8mm is soaked in a sodium hydroxide solution with a mass concentration of 60% at 55°C for 11h, filtered, washed with water, and treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber and sodium hydroxide solution is 1g:450mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the mixed dispersion, reacted at 90°C for 6h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and mixed dispersion is 1g:5g:220mL. The modified basalt fiber and the glass fiber with a length of 17 mm were added to the KH-570 silane coupling agent, reacted at 175° C. for 3 hours, filtered, and dried to obtain a modified basalt fiber-glass fiber composite material; wherein the mass ratio of the modified basalt fiber, the glass fiber, and the KH-570 silane coupling agent was 1:0.4:16.

[0058] Example 3

[0059] This embodiment provides a method for preparing a modified basalt fiber-glass fiber composite material, and the steps are as follows:

[0060] Nano-silicon dioxide and nano-ceramsite are dispersed in an ethanol aqueous solution with a mass concentration of 85% to obtain a mixed dispersion; wherein the mass volume ratio of nano-silicon dioxide, nano-ceramsite and ethanol aqueous solution is 1g:1g:120mL, the particle size of nano-silicon dioxide is 90nm, and the particle size of nano-ceramsite is 95nm. Basalt fiber with a length of 10mm is soaked in a sodium hydroxide solution with a mass concentration of 55% at 62°C for 10h, filtered, washed with water, and the treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber and sodium hydroxide solution is 1g:420mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the mixed dispersion, reacted at 88°C for 5h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of the treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and the mixed dispersion is 1g:5.5g:240mL. The modified basalt fiber and the glass fiber with a length of 14 mm were added to the KH-570 silane coupling agent, reacted at 168° C. for 2.5 h, filtered, and dried to obtain a modified basalt fiber-glass fiber composite material; wherein the mass ratio of the modified basalt fiber, the glass fiber, and the KH-570 silane coupling agent was 1:0.5:17.

[0061] Example 4

[0062] The present embodiment provides an artificial shellfish algae reef biological induction material, comprising the following components in parts by weight: 55 parts of steel slag powder with a particle size of 8 mm, 28 parts of sulfate cement, 45 parts of fly ash with a particle size of 150 mesh, 15 parts of cattle bone powder with a particle size of 5 mm, 20 parts of the modified basalt fiber-glass fiber composite material prepared in Example 1, and 12 parts of modified straw;

[0063] The preparation method of the modified straw comprises the following steps:

[0064] Add 180-mesh corn stalk powder to water, adjust the pH to 5.2, then add compound enzyme, soak at 55°C for 5h, filter, and obtain primary modified stalk powder; wherein the mass volume ratio of stalk powder to water is 1g:180mL, the compound enzyme is a mixed enzyme of cellulase and hemicellulase with a mass ratio of 1:0.7, the cellulase activity is 413.26U / g, the hemicellulase activity is 681.27U / g, and the mass ratio of stalk powder to compound enzyme is 1:0.013. Add primary modified stalk powder to potassium permanganate aqueous solution, react at 40°C for 2h, filter, wash with water, and dry to obtain modified stalk; the mass ratio of potassium permanganate in primary modified stalk powder and potassium permanganate aqueous solution is 1:4.

[0065] The preparation method of artificial shellfish algae reef biological induction material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them evenly, then adding water and stirring evenly, the water consumption is 343kg / m 3 , and obtain the artificial shellfish and algae reef biological induction material.

[0066] Example 5

[0067] The present embodiment provides an artificial shellfish and algae reef biological induction material, comprising the following components in parts by weight: 45 parts of steel slag powder with a particle size of 12 mm, 42 parts of sulfate cement, 30 parts of fly ash with a particle size of 180 mesh, 20 parts of cattle bone powder with a particle size of 10 mm, 16 parts of the modified basalt fiber-glass fiber composite material prepared in Example 2, and 18 parts of modified straw;

[0068] The preparation method of the modified straw comprises the following steps:

[0069] Add 220-mesh corn stalk powder to water, adjust the pH to 5.7, then add compound enzyme, soak at 52°C for 8 hours, filter, and obtain primary modified stalk powder; wherein the mass volume ratio of stalk powder to water is 1g:220mL, the compound enzyme is a mixed enzyme of cellulase and hemicellulase with a mass ratio of 1:0.9, the cellulase activity is 525.82U / g, the hemicellulase activity is 692.42U / g, and the mass ratio of stalk powder to compound enzyme is 1:0.018. Add primary modified stalk powder to potassium permanganate aqueous solution, react at 45°C for 3 hours, filter, wash with water, and dry to obtain modified stalk; the mass ratio of potassium permanganate in primary modified stalk powder and potassium permanganate aqueous solution is 1:6.

[0070] The preparation method of artificial shellfish algae reef biological induction material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them evenly, then adding water and stirring evenly, the water consumption is 414.5 kg / m 3, and obtain the artificial shellfish and algae reef biological induction material.

[0071] Example 6

[0072] The present embodiment provides an artificial shellfish algae reef biological induction material, comprising the following components in parts by weight: 50 parts of steel slag powder with a particle size of 10 mm, 30 parts of sulfate cement, 43 parts of fly ash with a particle size of 160 mesh, 30 parts of cattle bone powder with a particle size of 8 mm, 18 parts of the modified basalt fiber-glass fiber composite material prepared in Example 3, and 16 parts of modified straw;

[0073] The preparation method of the modified straw comprises the following steps:

[0074] Add 220-mesh corn stalk powder to water, adjust the pH to 5.5, then add compound enzyme, soak at 54°C for 6 hours, filter, and obtain primary modified stalk powder; wherein the mass volume ratio of stalk powder to water is 1g:200mL, the compound enzyme is a mixed enzyme of cellulase and hemicellulase with a mass ratio of 1:0.8, the cellulase activity is 485.67U / g, the hemicellulase activity is 644.29U / g, and the mass ratio of stalk powder to compound enzyme is 1:0.016. Add primary modified stalk powder to potassium permanganate aqueous solution, react at 42°C for 2.5 hours, filter, wash with water, and dry to obtain modified stalk; the mass ratio of potassium permanganate in primary modified stalk powder and potassium permanganate aqueous solution is 1:5.

[0075] The preparation method of artificial shellfish algae reef biological induction material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them evenly, then adding water and stirring evenly, the water consumption is 377.2 kg / m 3 , and obtain the artificial shellfish and algae reef biological induction material.

[0076] Comparative Example 1

[0077] This comparative example provides an artificial shellfish reef material, comprising the following components in parts by weight: 55 parts of steel slag powder with a particle size of 8 mm, 28 parts of sulfate cement, 45 parts of fly ash with a particle size of 150 mesh, 15 parts of cattle bone powder with a particle size of 5 mm, 20 parts of modified basalt fiber-glass fiber composite material, and 12 parts of modified reed;

[0078] The preparation method of the modified basalt fiber-glass fiber composite material comprises the following steps:

[0079] Nano-silicon dioxide and nano-ceramsite are dispersed in an ethanol aqueous solution with a mass concentration of 90% to obtain a mixed dispersion; wherein the mass volume ratio of nano-silicon dioxide, nano-ceramsite and ethanol aqueous solution is 1g:0.8g:110mL, the particle size of nano-silicon dioxide is 80nm, and the particle size of nano-ceramsite is 100nm. Basalt fiber with a length of 12mm is soaked in a sodium hydroxide solution with a mass concentration of 50% at 70°C for 9h, filtered, washed with water, and treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber and sodium hydroxide solution is 1g:400mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the mixed dispersion, reacted at 85°C for 4h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and mixed dispersion is 1g:6g:260mL. The modified basalt fiber and the glass fiber with a length of 14 mm are added to the KH-570 silane coupling agent, reacted at 165° C. for 2 hours, filtered, and dried to obtain the modified basalt fiber-glass fiber composite material; wherein the mass ratio of the modified basalt fiber, the glass fiber, and the KH-570 silane coupling agent is 1:0.6:20.

[0080] The preparation method of modified reed comprises the following steps:

[0081] Add 180-mesh reeds into water, adjust the pH to 5.2, then add composite enzymes, soak at 55°C for 5 hours, filter, and obtain primary modified reeds; wherein, the mass volume ratio of reeds to water is 1g:180mL, the composite enzyme is a mixed enzyme of cellulase and hemicellulase in a mass ratio of 1:0.7, the cellulase activity is 413.26U / g, the hemicellulase activity is 681.27U / g, and the mass ratio of reeds to composite enzymes is 1:0.013; add primary modified reeds into potassium permanganate aqueous solution, react at 40°C for 2 hours, filter, wash with water, and dry to obtain modified reeds; the mass ratio of potassium permanganate in primary modified reeds and potassium permanganate aqueous solution is 1:4.

[0082] The preparation method of artificial shellfish reef material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified reed, mixing them evenly, then adding water and stirring evenly, the water consumption is 343kg / m 3 , and obtain the artificial shellfish and algae reef material.

[0083] Comparative Example 2

[0084] This comparative example provides an artificial shellfish reef material, comprising the following components in parts by weight: 55 parts of steel slag powder with a particle size of 8 mm, 28 parts of sulfate cement, 45 parts of fly ash with a particle size of 150 mesh, 15 parts of cattle bone powder with a particle size of 5 mm, 20 parts of modified basalt fiber, and 12 parts of modified straw;

[0085] The preparation method of modified basalt fiber comprises the following steps:

[0086] Nano-silicon dioxide and nano-ceramsite are dispersed in an ethanol aqueous solution with a mass concentration of 90% to obtain a mixed dispersion; wherein the mass volume ratio of nano-silicon dioxide, nano-ceramsite and ethanol aqueous solution is 1g:0.8g:110mL, the particle size of nano-silicon dioxide is 80nm, and the particle size of nano-ceramsite is 100nm. Basalt fiber with a length of 12mm is soaked in a sodium hydroxide solution with a mass concentration of 50% at 70°C for 9h, filtered, washed with water, and treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber and sodium hydroxide solution is 1g:400mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the mixed dispersion, reacted at 85°C for 4h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and mixed dispersion is 1g:6g:260mL.

[0087] The steps of the preparation method of modified straw are as follows:

[0088] Add 180-mesh corn stalk powder to water, adjust the pH to 5.2, then add compound enzyme, soak at 55°C for 5h, filter, and obtain primary modified stalk powder; wherein the mass volume ratio of stalk powder to water is 1g:180mL, the compound enzyme is a mixed enzyme of cellulase and hemicellulase with a mass ratio of 1:0.7, the cellulase activity is 413.26U / g, the hemicellulase activity is 681.27U / g, and the mass ratio of stalk powder to compound enzyme is 1:0.013. Add primary modified stalk powder to potassium permanganate aqueous solution, react at 40°C for 2h, filter, wash with water, and dry to obtain modified stalk; the mass ratio of potassium permanganate in primary modified stalk powder and potassium permanganate aqueous solution is 1:4.

[0089] The preparation method of artificial shellfish algae reef material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber and modified straw, mixing them evenly, then adding water and stirring evenly, the water consumption is 343kg / m 3 , and obtain the artificial shellfish and algae reef material.

[0090] Comparative Example 3

[0091] This comparative example provides an artificial shellfish reef material, comprising the following components in parts by weight: 55 parts of steel slag powder with a particle size of 8 mm, 28 parts of sulfate cement, 45 parts of fly ash with a particle size of 150 mesh, 15 parts of cattle bone powder with a particle size of 5 mm, 20 parts of modified basalt fiber-glass fiber composite material, and 12 parts of modified straw;

[0092] The preparation method of the modified basalt fiber-glass fiber composite material comprises the following steps:

[0093] Nano-silicon dioxide is dispersed in an ethanol aqueous solution with a mass concentration of 90% to obtain a dispersion; wherein the mass volume ratio of nano-silicon dioxide to the ethanol aqueous solution is 1.8g:110mL, and the particle size of nano-silicon dioxide is 80nm. Basalt fiber with a length of 12mm is soaked in a sodium hydroxide solution with a mass concentration of 50% at 70°C for 9h, filtered, washed with water, and treated basalt fiber is obtained; wherein the mass volume ratio of basalt fiber to sodium hydroxide solution is 1g:400mL. The treated basalt fiber and vinyl tri(β-methoxyethoxy) silane are added to the dispersion, reacted at 85°C for 4h, filtered, washed with water, and dried to obtain modified basalt fiber; wherein the mass volume ratio of the treated basalt fiber, vinyl tri(β-methoxyethoxy) silane and the mixed dispersion is 1g:6g:260mL. The modified basalt fiber and the glass fiber with a length of 14 mm were added to the KH-570 silane coupling agent, reacted at 165° C. for 2 h, filtered, and dried to obtain a modified basalt fiber-glass fiber composite material; wherein the mass ratio of the modified basalt fiber, the glass fiber, and the KH-570 silane coupling agent was 1:0.6:20.

[0094] The steps of the preparation method of modified straw are as follows:

[0095] Add 180-mesh corn stalk powder to water, adjust the pH to 5.2, then add compound enzyme, soak at 55°C for 5h, filter, and obtain primary modified stalk powder; wherein the mass volume ratio of stalk powder to water is 1g:180mL, the compound enzyme is a mixed enzyme of cellulase and hemicellulase with a mass ratio of 1:0.7, the cellulase activity is 413.26U / g, the hemicellulase activity is 681.27U / g, and the mass ratio of stalk powder to compound enzyme is 1:0.013. Add primary modified stalk powder to potassium permanganate aqueous solution, react at 40°C for 2h, filter, wash with water, and dry to obtain modified stalk; the mass ratio of potassium permanganate in primary modified stalk powder and potassium permanganate aqueous solution is 1:4.

[0096] The preparation method of artificial shellfish reef material comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them evenly, then adding water and stirring evenly, the water consumption is 343kg / m 3 , and obtain the artificial shellfish and algae reef material.

[0097] Test Example 1

[0098] The compressive strength, porosity, abrasion and the amount of algae and oyster larvae attached to the artificial shellfish algae reef biological induction materials of Examples 4-6 and the artificial shellfish algae reef materials of Comparative Examples 1-3 were tested, and the specific testing standards are as follows:

[0099] Compressive strength: refer to GB / T 50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the artificial shellfish and algae reef biological induction materials of Examples 4-6 and the artificial shellfish and algae reef materials of Comparative Examples 1-3 were cured for 28 days, immersed in seawater for 60 days, and then taken out to test the compressive strength;

[0100] Porosity: The artificial shellfish algae reef biological induction materials of Examples 4-6 and the artificial shellfish algae reef materials of Comparative Examples 1-3 were made into 150*150*150mm concrete specimens, cured for 28 days, taken out, put into a dryer for drying for 24 hours, and weighed the mass m0 after drying the water; then put it into water and soak it for 2 days, took it out, weighed the mass m1, and calculated the porosity (e) according to the following formula:

[0101]

[0102] Abrasion rate: The artificial shellfish reef biological induction materials of Examples 4-6 and the artificial shellfish reef materials of Comparative Examples 1-3 were made into 150*150*150mm concrete specimens, cured for 28 days, taken out, put into a dryer for drying for 24 hours, and weighed after drying the water content m3, and then washed with a water flow at a speed of 3.5m / s. After 60 days, the specimens were taken out and put into a dryer for drying for 24 hours. The mass of the artificial shellfish reef after washing was m4. The abrasion loss (g) was calculated according to the following formula:

[0103] Wear rate (%) = [(m3-m4) / m3] × 100%;

[0104] Attachment amount of macroalgae and oyster larvae: The artificial shellfish algae reef biological induction materials of Examples 4-6 and Comparative Examples 1-3 were made into 30cm×30cm×5cm hanging boards, which were placed in seawater in September 2023. After 30 days, the test hanging boards in the water were lifted out of the water to conduct quantitative analysis of macroalgae and oyster larvae per unit area;

[0105] The specific test results are shown in Table 1:

[0106] Table 1 Material properties of Examples 4-6 and Comparative Examples 1-3

[0107]

[0108]

[0109] As can be seen from Table 1, the present invention selects steel slag powder, sulfate cement, fly ash, cattle bone meal, modified basalt fiber-glass fiber composite material and modified straw as the basic materials of artificial shellfish reefs. Several raw materials have a composite reinforcement effect, which jointly improves the strength, corrosion resistance and scour resistance of the artificial shellfish reef, and solves the problem of poor attachment effect of large algae and oyster larvae.

[0110] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a modified basalt fiber-glass fiber composite material, characterized in that: The steps include: Nano silicon dioxide and nano ceramsite are dispersed in an alcohol solution to obtain a mixed dispersion; basalt fiber is immersed in a strong alkaline solution to obtain treated basalt fiber; the treated basalt fiber and vinyl tri(β-methoxyethoxy)silane are added to the mixed dispersion to react to obtain modified basalt fiber; the modified basalt fiber and glass fiber are coupled to obtain the modified basalt fiber-glass fiber composite material.

2. The method for preparing the modified basalt fiber-glass fiber composite material according to claim 1, characterized in that: The mass volume ratio of the nano silicon dioxide, nano ceramsite and alcohol solution is 1g: 0.8-1.2g: 110-130mL.

3. The method for preparing the modified basalt fiber-glass fiber composite material according to claim 1, characterized in that: The basalt fiber is immersed in the strong alkaline solution at a temperature of 55 to 70° C. and a soaking time of 9 to 11 hours.

4. The method for preparing the modified basalt fiber-glass fiber composite material according to claim 1, characterized in that: The reaction temperature is 85-90° C., and the reaction time is 4-6 hours.

5. The method for preparing the modified basalt fiber-glass fiber composite material according to claim 1, characterized in that: The coupling method comprises: adding the modified basalt fiber and the glass fiber into a coupling agent, and reacting at 165-175° C. for 2-3 hours.

6. The modified basalt fiber-glass fiber composite material prepared by the preparation method according to any one of claims 1 to 5.

7. An artificial shellfish and algae reef biological induction material, characterized in that: The invention comprises the following components in parts by weight: 45 to 55 parts of steel slag powder, 28 to 42 parts of sulfate cement, 30 to 45 parts of fly ash, 15 to 30 parts of cattle bone powder, 16 to 20 parts of the modified basalt fiber-glass fiber composite material according to claim 6, and 12 to 18 parts of modified straw; The modified straw is prepared by enzymatic hydrolysis and oxidation of the straw.

8. The artificial shellfish and algae reef biological induction material according to claim 7, characterized in that: The enzymes for enzymolysis include cellulase and hemicellulase.

9. The method for preparing the artificial shellfish and algae reef biological induction material according to any one of claims 7 to 8, characterized in that: The method comprises the following steps: weighing steel slag powder, sulfate cement, fly ash, cattle bone powder, modified basalt fiber-glass fiber composite material and modified straw, mixing them, adding water and stirring to obtain the artificial shellfish algae reef biological induction material.

10. Use of the method for preparing the modified basalt fiber-glass fiber composite material according to any one of claims 1 to 5, or the modified basalt fiber-glass fiber composite material according to claim 6, or the artificial shellfish and algae reef biological induction material according to any one of claims 7 to 8, or the method for preparing the artificial shellfish and algae reef biological induction material according to claim 9 in preparing artificial reefs and / or constructing artificial shellfish and algae reef habitats.

Citation Information

Cited By

  • Low-carbon anti-crack concrete and preparation method thereof

    CN120172701A

  • Low-carbon anti-cracking concrete and preparation method thereof

    CN120172701B