Preparation method and application of high-strength stone-like water permeable brick

By adding fibers and resin to imitation stone permeable bricks, the amount of cement is reduced, and uniform particle aggregate and high-temperature firing technology is used to solve the contradiction between the strength and permeability of traditional imitation stone permeable bricks, and high-strength, good permeability and Preparation of beautiful imitation stone permeable bricks.

CN119038958AInactive Publication Date: 2024-11-29GUANGDONG MEILV ENVIRONMENTAL PROTECTION TECH MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410783268.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When traditional imitation stone permeable bricks increase their strength, the increase in cement content will affect the permeable performance, and lead to unclear imitation stone patterns and affect their aesthetics.

Method used

By adding fibers and resin to the raw materials of stone-imitated permeable bricks, the strength and adhesion of the bricks are improved, the amount of cement is reduced, and uniform particle aggregate and high-temperature firing technology are used to ensure the formation and cross-stability of permeable gaps, combined with vibration Mold forming technology forms uniform and permeable gaps and clear imitation stone patterns.

Benefits of technology

The preparation of high-strength permeable bricks is realized, which avoids the risks of cracking and fracture, ensures the permeable performance and beauty, improves the compressive strength and permeability coefficient of imitation stone permeable bricks, and maintains the clearness of imitation stone patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038958A_ABST
    Figure CN119038958A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of water permeable brick manufacturing, in particular to a preparation method and application of a high-strength stone-like water permeable brick, cement and aggregate are taken and put into stirring equipment, solid raw materials are pre-mixed, after the solid raw materials are mixed, water is added for further stirring and mixing, and in the raw material mixing process of a base material, the raw materials are uniformly mixed; the preparation method comprises the following steps: adding a cementing material and a reinforcing agent into stirring equipment, stirring and mixing the cementing material and the reinforcing agent with the raw materials to obtain a bottom material stirring mixture, putting white cement and sand into the stirring equipment, premixing, adding the cementing material, fibers, the reinforcing agent, resin, a stone-like agent and water, and mixing and stirring to obtain a surface material stirring mixture. According to the preparation method and application of the high-strength stone-like water permeable brick, the fiber and the resin are added into the raw materials of the water permeable brick, the fiber can provide strength for the water permeable brick, and the resin can enable the backing material and the surface material of the stone-like water permeable brick to have better binding power, so that the strength of the water permeable brick is improved, and the risk of cracking and fracture is not prone to occurring; the preparation strength of the stone-like water permeable brick is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of permeable brick manufacturing, in particular to a preparation method and application of high-strength stone-imitation permeable brick. Background Art

[0002] Permeable bricks are a new type of green and environmentally friendly building material. Its raw materials mainly include environmentally friendly materials such as cement, sand, slag and fly ash. Permeable bricks have good permeability, anti-slip function, good wear resistance, natural and lasting color, long service life, smooth appearance, clear edges and corners, neat lines, frost resistance, high salt and alkali resistance and not easy to break. The compressive and flexural strength are also higher than similar products. In addition, permeable bricks have low maintenance costs and are easy to replace, so it is convenient to bury pipelines under the road surface. As the name suggests, imitation stone permeable bricks are permeable bricks with stone surface texture. The emergence of imitation stone permeable bricks can not only replace natural stone, but also add strength to the construction of sponge cities, solving the problem of using stone while failing to meet the permeable function.

[0003] In the process of production and preparation of imitation stone permeable bricks, the traditional process of imitation stone permeable bricks generally increases the amount of cement to achieve the improvement of the strength of the permeable bricks. The higher the cement content, the higher the strength. However, the increase in cement content will affect the water permeability of the permeable bricks, while the low cement content will cause the strength of the permeable bricks to be low. In addition, the increase in cement content will also cause other fillers of the permeable bricks to be unclear, resulting in unclear imitation stone patterns of the permeable bricks, affecting the beauty of the imitation stone permeable bricks. Summary of the invention

[0004] The purpose of the present invention is to provide a preparation method and application of high-strength stone-like permeable bricks to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: the permeable brick includes a base material and a surface material, and the base material of the permeable brick includes the following raw materials:

[0006] 300-350 parts of cement, 450-500 parts of aggregate, 50-80 parts of binder, 20-40 parts of reinforcing agent, 40-50 parts of fiber and 10-20 parts of water;

[0007] The fabric of the permeable brick includes the following raw materials:

[0008] 100-150 parts of white cement, 60-90 parts of sand, 30-40 parts of binder, 30-50 parts of fiber, 10-15 parts of reinforcing agent, 5-15 parts of resin, 5-8 parts of stone-like agent and 5-10 parts of water;

[0009] The preparation of the permeable brick comprises the following steps:

[0010] S1. Base material configuration: Take cement and aggregate and put them into a mixing device, pre-mix the solid raw materials, and after the solid raw materials are mixed, add water to further mix them. During the mixing process of the base material raw materials, add a binder and a reinforcing agent to the mixing device and mix them with the raw materials to obtain a base material mixing compound;

[0011] S2. Fabric configuration: white cement and sand are put into a mixing device for premixing, and then a binder, fiber, reinforcing agent, resin, stone-like agent and water are added and mixed to obtain a fabric mixing material;

[0012] S3. Molding: pouring the base material mixture into the mold and vibrating the mold, then squeezing the base material mixture in the mold with a pressing plate, adding the surface material mixture to the surface of the base material mixture after compaction, and vibrating the mold, and then closing the mold and pressurizing it to obtain a formed wet blank;

[0013] S4. Curing: Place the wet blank of the permeable brick into the curing room and let it stand, watering it regularly during the standing period;

[0014] S5. Firing: The cured blank is placed in a firing kiln and then fired at high temperature to obtain a finished permeable brick;

[0015] S6. Cooling: After firing, the finished permeable bricks are placed in a cooling room for natural cooling and watered after cooling.

[0016] In a further embodiment, the aggregate is one or more of gravel, crushed stone, quartz sand, expanded clay and tailings, and the aggregate particles are 20-40 meshes. By uniformly sized aggregates, the aggregates can imitate stones to form a stone-like effect, and the uniformly sized aggregates can effectively ensure the formation of permeable gaps and the cross stability between the gaps of permeable bricks during the production process.

[0017] In a further embodiment, the fibers include carbon fibers and bamboo fibers, and the resin is polyurethane resin, which is a water-permeable resin. Adding the water-permeable resin can allow the base material and the surface material of the permeable brick to be fully bonded, thereby improving the bonding strength of the two parts. Both carbon fibers and bamboo fibers are high-strength fibers. The high-strength fibers are mixed in the raw materials and crisscrossed with each other, which can effectively improve the tear stress resistance of the permeable brick, thereby improving the strength of the imitation stone permeable brick.

[0018] In a further embodiment, the temperature in the curing room is 20-30° C., the humidity in the room is 75%-90%, and the wet blank is cured in the curing room for 7 days.

[0019] In a further embodiment, the firing temperature in S5 is 1430-1450°C, the firing time is 3-4h, and the finished permeable brick is kept warm for 15h after firing, and the insulation temperature is 60-100°C.

[0020] In a further embodiment, the mold closing pressure in S3 is 15MPa, and the vibration frequency of the mold is 100Hz. Through high-speed vibration, the raw materials can be vibrated and compacted to form stable water-permeable gaps. During subsequent mold closing and pressing, there will be no uneven water-permeable gaps. Therefore, the permeable bricks can have more uniform and efficient water-permeable performance after being formed.

[0021] In a further embodiment, the reinforcing agent is composed of ethylene oxide, propylene oxide and azodicarbonamide, and the component ratios are 20%-25% azodicarbonamide, 30%-35% propylene oxide and 50%-55% azodicarbonamide respectively. By reinforcing the raw materials of the permeable bricks with the reinforcing agent, the strength of the permeable bricks can be effectively improved.

[0022] In a further embodiment, the ratio of the reinforcing agent added to the base material and the outer material is 1:0.4, and the ratio of the fiber added to the base material and the outer material is 1:0.8.

[0023] In a further embodiment, the fiber is obtained by twisting monofilament fiber into strands, and the fiber is evenly cut by a cutting machine after being obtained. The length of the fiber is 3-5 cm. The fiber is cut into uniform lengths, and after being mixed into the raw materials, the fibers are staggered with each other. The high tensile strength of the fiber is utilized to improve the strength of the permeable brick, which can effectively reduce the breakage and crushing of the permeable brick, thereby ensuring that the service life of the permeable brick is increased.

[0024] Permeable bricks are used for paving roads and paved areas.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention adds fiber and resin to the raw material of the imitation stone permeable brick. The fiber can provide strength for the imitation stone permeable brick, and the resin can make the base material and the surface material of the imitation stone permeable brick have better bonding force, so that the strength of the permeable brick is improved. Therefore, the imitation stone permeable brick has stronger molding strength after molding, and is not prone to cracking and breaking risks, thereby ensuring the strength of the imitation stone permeable brick.

[0027] 2. The present invention improves the strength of the imitation stone permeable brick by adding fiber and resin, without increasing the amount of cement in the permeable brick. Therefore, the imitation stone permeable brick does not increase the amount of cement in order to increase the strength. The produced imitation stone permeable brick will not have unclear imitation stone texture on the surface due to the increase in the amount of cement, ensuring that the texture of the imitation stone aggregate is clear, making the imitation stone permeable brick beautiful in appearance;

[0028] 3. In the present invention, during the preparation process of the base material and the surface material of the imitation stone permeable brick, after the base material and the surface material are stirred, the base material is first poured into the mold, and the mold is vibrated so that the base material in the mold can be fully and evenly spread, so that a stable permeable gap is formed between the raw materials, and then the surface material is poured onto the base material of the mold, vibrated again, and finally the mold is closed to press and form. During pressing, because the base material and the surface material are both flattened, the mold is closed to bond the surface material and the base material to each other. During the process, the permeable gap shrinks regularly to form a stable brick blank, and the permeable gap is evenly distributed. Compared with directly pouring the base material and the surface material for pressing and forming, there will be uneven extrusion of the mixture, resulting in uneven permeable gaps, affecting the subsequent permeable effect, and the problem of unsightly imitation stone texture will also occur. Therefore, through the above-mentioned molding method, the strength of the imitation stone permeable brick can be guaranteed while ensuring the beauty and permeability of the permeable brick. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the process framework of the preparation method of the present invention. DETAILED DESCRIPTION

[0030] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The following is combined with Figure 1 The application is further described with examples;

[0032] Embodiment 1

[0033] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0034] 1) Base material raw materials: 150kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 10kg fiber and 25kg water;

[0035] Fabric materials: 60kg white cement, 30kg sand, 8kg binder, 8kg fiber, 5kg reinforcing agent, 5kg resin, 2.5kg stone-like agent and 15kg water;

[0036] Base material configuration: 150kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 10kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0037] Fabric configuration: 60kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 8kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 5kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0038] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0039] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0040] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0041] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0042] The finished product of imitation stone permeable brick has a compressive strength of 60MPa, a water permeability coefficient of 30L / m / h, and a bonding strength between the surface layer and the base layer of 3.8×104. The imitation stone permeable brick has an excellent texture.

[0043] Embodiment 2

[0044] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0045] 1) Base material raw materials: 200kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 10kg fiber and 25kg water;

[0046] Fabric materials: 80kg white cement, 30kg sand, 8kg binder, 8kg fiber, 5kg reinforcing agent, 5kg resin, 2.5kg stone-like agent and 15kg water;

[0047] Base material configuration: 200kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 10kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0048] Fabric configuration: 80kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 8kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 5kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0049] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0050] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0051] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0052] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0053] The finished product of imitation stone permeable brick has a compressive strength of 63MPa, a permeability coefficient of 33L / m / h, and a bonding strength between the surface layer and the base layer of 4×104. The imitation stone permeable brick meets the standards, but the increase in cement content causes the aesthetics of the imitation stone permeable brick to decline and the permeability is poor.

[0054] It can be seen from the above-mentioned Example 1 and Example 2 that when the imitation stone permeable brick is prepared, the cement and white cement content of the base material and the surface material is adjusted to improve the strength of the brick body. However, such strength improvement has limitations, and a larger cement and white cement content will cause the imitation stone effect of the imitation stone permeable brick to be unclear.

[0055] Embodiment 3

[0056] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0057] 1) Base material raw materials: 130kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 15kg fiber and 25kg water;

[0058] Fabric materials: 50kg white cement, 30kg sand, 8kg binder, 15kg fiber, 5kg reinforcing agent, 8kg resin, 2.5kg stone-like agent and 15kg water;

[0059] Base material configuration: 130kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 15kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0060] Fabric configuration: 50kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 15kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 8kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0061] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0062] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0063] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0064] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0065] The finished product of imitation stone permeable brick has a compressive strength of 65MPa, a water permeability coefficient of 35L / m / h, a bonding strength between the surface layer and the base layer of 4.2×104, and the imitation stone permeable brick has an excellent texture.

[0066] Embodiment 4

[0067] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0068] 1) Base material raw materials: 120kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 30kg fiber and 25kg water;

[0069] Fabric materials: 45kg white cement, 30kg sand, 8kg binder, 20kg fiber, 5kg reinforcing agent, 10kg resin, 2.5kg stone-like agent and 15kg water;

[0070] Base material configuration: 120kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 30kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0071] Fabric configuration: 45kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 20kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 10kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0072] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0073] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0074] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0075] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0076] The finished product of imitation stone permeable brick has a compressive strength of 75MPa, a water permeability coefficient of 37L / m / h, a bonding strength between the surface layer and the base layer of 4.6×104, and the imitation stone permeable brick has an excellent texture.

[0077] According to the comparison between Example 3 and Example 4 and Example 1, it can be seen that by reducing the addition amount of cement and white cement, but increasing the addition amount of fiber and resin, the comparative strength and water permeability coefficient have a significant increase. The reduction in the content of cement and white cement reduces the amount of raw materials for the base material and the surface material, thereby increasing the permeable gap and improving the water permeability. At the same time, the fiber increases the strength of the brick body, ensuring that the strength is improved while the water permeability is also improved. In addition, reducing the addition amount of cement and white cement will also reduce the impact on the imitation stone texture, ensuring that the imitation stone texture of the imitation stone permeable brick is clear and beautiful.

[0078] Embodiment 5

[0079] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0080] 1) Base material raw materials: 150kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 15kg fiber and 25kg water;

[0081] Fabric materials: 60kg white cement, 30kg sand, 8kg binder, 15kg fiber, 5kg reinforcing agent, 8kg resin, 2.5kg stone-like agent and 15kg water;

[0082] Base material configuration: 150kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 15kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0083] Fabric configuration: 60kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 15kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 8kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0084] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0085] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0086] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0087] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0088] The finished product of imitation stone permeable brick has a compressive strength of 80MPa, a water permeability coefficient of 40L / m / h, a bonding strength between the surface layer and the base layer of 4.4×104, and the imitation stone permeable brick has an excellent texture.

[0089] Embodiment 6

[0090] This embodiment provides a stone-like ceramic permeable brick, and the preparation method thereof comprises the following steps:

[0091] 1) Base material raw materials: 150kg cement, 200kg aggregate, 15kg binder, 5kg reinforcing agent, 20kg fiber and 25kg water;

[0092] Fabric materials: 60kg white cement, 30kg sand, 8kg binder, 18kg fiber, 5kg reinforcing agent, 12kg resin, 2.5kg stone-like agent and 15kg water;

[0093] Base material configuration: 150kg of cement and 200kg of aggregate are conveyed to the mixing equipment through the conveying device, the mixer is started to mix the solid cement and aggregate, and then 5kg of water is added to continue mixing, and then 15kg of binder, 5kg of reinforcing agent and 20kg of fiber are added to the mixing equipment respectively, and then 20kg of water is added to continue mixing to obtain the base material mixing material;

[0094] Fabric configuration: 60kg of white cement and 30kg of sand are transported to the mixing equipment through the conveying device for mixing, and the mixer is started to mix the solid white cement and sand. After the solids are mixed evenly, 2.5kg of water is added, and then 8kg of binder, 18kg of fiber, 5kg of reinforcing agent, 2.5kg of stone-like agent, 12kg of resin and 12.5kg of water are added to the mixing equipment for mixing to obtain the fabric mixing material;

[0095] 2) Molding: pour the base material mixture into the mold and vibrate the mold, then use a pressing plate to squeeze the base material mixture in the mold, add the surface material mixture to the surface of the base material mixture in the mold after compaction, and vibrate the mold, then close the mold and pressurize it to obtain a formed wet blank;

[0096] 3) Curing: Place the wet blank of the permeable brick in the curing room and let it stand, watering it regularly during the standing period;

[0097] 4) Firing: Put the cured blank into the firing kiln, and then sinter it at high temperature to obtain the finished permeable brick;

[0098] 5) Cooling: After the fired permeable bricks are finished, place them in a cooling room to cool naturally, and then water them after cooling.

[0099] The finished product of imitation stone permeable brick has a compressive strength of 85MPa, a permeability coefficient of 43L / m / h, and a bonding strength between the surface layer and the bottom layer of 5×104. The imitation stone permeable brick has excellent texture. By changing the amount of resin added, the bonding strength of the base material and the surface material can be improved, thereby improving the bonding strength of the imitation stone permeable brick, ensuring that the base material and the surface material after the imitation stone permeable brick is prepared are more stably bonded.

[0100] According to the comparison between Example 5 and Example 6 and Example 1, it can be seen that while keeping the addition amount of cement and white cement unchanged, increasing the addition amount of fiber and resin, the comparative strength and water permeability coefficient are significantly increased, which can provide stronger strength guarantee for the stone-proof permeable bricks, and the mold bonding force between the base material and the surface material is stronger.

[0101] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing high-strength imitation stone permeable bricks, characterized in that: The permeable brick includes a base material and a surface material. The base material of the permeable brick includes the following raw materials: 300-350 parts of cement, 450-500 parts of aggregate, 50-80 parts of binder, 20-40 parts of reinforcing agent, 40-50 parts of fiber and 10-20 parts of water; The fabric of the permeable brick includes the following raw materials: 100-150 parts of white cement, 60-90 parts of sand, 30-40 parts of binder, 30-50 parts of fiber, 10-15 parts of reinforcing agent, 5-15 parts of resin, 5-8 parts of stone-like agent and 5-10 parts of water; The preparation of the permeable brick comprises the following steps: S1. Base material configuration: Take cement and aggregate and put them into a mixing device, pre-mix the solid raw materials, and after the solid raw materials are mixed, add water to further mix them. During the mixing process of the base material raw materials, add a binder and a reinforcing agent to the mixing device and mix them with the raw materials to obtain a base material mixing compound; S2. Fabric configuration: white cement and sand are put into a mixing device for premixing, and then a binder, fiber, reinforcing agent, resin, stone-like agent and water are added and mixed to obtain a fabric mixing material; S3. Molding: pouring the base material mixture into the mold and vibrating the mold, then squeezing the base material mixture in the mold with a pressing plate, adding the surface material mixture to the surface of the base material mixture after compaction, and vibrating the mold, and then closing the mold and pressurizing it to obtain a formed wet blank; S4. Curing: Place the wet blank of the permeable brick into the curing room and let it stand, watering it regularly during the standing period; S5. Firing: The cured blank is placed in a firing kiln and then fired at high temperature to obtain a finished permeable brick; S6. Cooling: After firing, the finished permeable bricks are placed in a cooling room for natural cooling and watered after cooling.

2. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The aggregate is one or more of gravel, crushed stone, quartz sand, ceramsite and tailings, and the particles of the aggregate are 20-40 meshes.

3. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The fibers include carbon fibers and bamboo fibers, and the resin is polyurethane resin.

4. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The temperature in the curing room is 20-30° C., the humidity in the room is 75%-90%, and the wet blank is cured in the curing room for 7 days.

5. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The firing temperature in S5 is 1430-1450°C, the firing time is 3-4h, and the finished permeable brick is kept warm for 15h after firing, and the insulation temperature is 60-100°C.

6. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The mold clamping pressure of the mold in S3 is 15 MPa, and the vibration frequency of the mold is 100 Hz.

7. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The reinforcing agent is composed of ethylene oxide, propylene oxide and azodicarbonamide, and the proportions of the components are respectively 20%-25% of azodicarbonamide, 30%-35% of propylene oxide and 50%-55% of azodicarbonamide.

8. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The ratio of the reinforcing agent added to the base material and the outer material is 1:0.4, and the ratio of the fiber added to the base material and the outer material is 1:0.

8.

9. The method for preparing a high-strength imitation stone permeable brick according to claim 1, characterized in that: The fiber is obtained by twisting monofilament fibers into strands. After the fiber is obtained, it is evenly cut by a cutting machine. The length of the fiber is 3-5 cm.

10. The permeable bricks according to any one of claims 1 to 9 are used for paving roads and paving sites.