Water-based flexible glue for improving softness and processability of hard carbon negative pole piece, hard carbon negative pole piece and preparation method of hard carbon negative pole piece

By using a combination of specific aqueous soft glue and PAA-type water-based adhesives in the hard carbon negative electrode sheet, the problem of hard brittleness and cracking of the hard carbon negative electrode sheet during processing is solved, and its softness and processing performance are significantly improved. , suitable for sodium ion battery applications.

CN119039505AActive Publication Date: 2024-11-29BLUE OCEAN & BLACK STONE TECH CO LTD (FUJIAN)

Patent Information

Application Number
CN202411107766.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing hard carbon negative electrode sheets are prone to hard brittle, cracking and material dropping during processing, and it is difficult to take into account both stability and processing performance.

Method used

The aqueous soft glue obtained by mixing the polymerization reaction of a specific first monomer and the second monomer with a PAA-type aqueous binder is used to form a low glass transition temperature by using the surfactant and a protective colloid stabilizer emulsion. Flexible glue is used to improve the softness and processing performance of hard carbon negative electrode sheets.

Benefits of technology

It significantly improves the softness and processing performance of hard carbon negative electrode sheets, avoids hard brittleness and cracking problems, and maintains high adhesion and cohesion. It is suitable for the preparation of hard carbon negative electrode sheets for sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991310890000051
    Figure BDA0004991310890000051
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of sodium-ion battery hard carbon negative pole pieces, and particularly discloses water-based flexible glue for improving softness and processability of a hard carbon negative pole piece, the hard carbon negative pole piece and a preparation method of the hard carbon negative pole piece. The invention discloses water-based flexible glue for improving softness and processability of a hard carbon negative pole piece. The water-based flexible glue is obtained by mixing and polymerizing a plurality of first monomers and a plurality of second monomers. The general formula of the first monomer is CH2 = CR1R2, R1 is one of H and C1-C4 alkyl groups, and R2 is one of functional groups of-CONH2,-CONHCH3,-CONHCH2CH3,-CONN (CH3) 2,-CONHCH2OH,-CONHCH2OH and-CONHCH2CH2OH. The general formula of the first monomer is CH2 = CR1R2, R1 is one of H and C1-C4 alkyl groups, and R2 is one of functional groups of-CONH2,-CONHCH3,-CONHCH2CH3,-CONHCH2CH3,-CONHCH2CH2OH and-CONHCH2CH2OH. The general formula of the second monomer is CH2 = CHCOOR3, and R3 is selected from C2-C18 alkyl groups or C2-C18 alkyl groups substituted by hydroxyl groups. When the water-based flexible glue is synthesized, the molar ratio of the second monomer is greater than 50%. When the aqueous flexible glue and a polyacrylic acid aqueous adhesive are used together for preparing a hard carbon negative pole piece, the stability and the processability of the pole piece can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of hard carbon negative electrode sheets for sodium ion batteries, and in particular to a water-based soft gel for improving the softness and processing performance of hard carbon negative electrode sheets, a hard carbon negative electrode sheet and a preparation method thereof. Background Art

[0002] Hard carbon is a type of carbon that will not graphitize after high-temperature treatment. Its internal crystal arrangement is disordered and the interlayer spacing is large, which allows the hard carbon negative electrode to store more charge in the same volume, thereby improving the energy density and endurance of the battery.

[0003] Hard carbon materials are widely used as negative electrode materials for sodium-ion batteries due to their high capacity and good rate performance. However, for the preparation process of hard carbon negative electrode sheets, how to ensure the stability and processing performance of the sheets becomes the key. At present, the CMC (carboxymethyl cellulose) + SBR (styrene-butadiene rubber) system is a commonly used adhesive, but it has limitations in the dispersibility and adhesion of hard carbon particles.

[0004] PAA (polyacrylic acid) water-based adhesives have good affinity for hard carbon particles due to their rich functional groups, such as ester groups and cyano groups, and can effectively disperse hard carbon particles and provide good adhesion. However, due to the high Tg (glass transition temperature) of PAA-based water-based adhesives, the hard carbon negative electrode sheets made are often hard and brittle, which leads to problems such as cracking and falling off during processing.

[0005] Currently, there is no effective solution that can simultaneously take into account the stability and processing performance of hard carbon negative electrode sheets. Summary of the invention

[0006] In view of the above problems, this application proposes the following technical solutions.

[0007] In a first aspect, the present application proposes a water-based soft glue for improving the softness and processing performance of hard carbon negative electrode sheets, and adopts the following technical solution.

[0008] A water-based soft glue for improving the softness and processing performance of a hard carbon negative electrode sheet. The water-based soft glue is obtained by a mixed polymerization reaction of several first monomers and several second monomers.

[0009] The first monomer has a general formula of CH2=CR1R2, wherein R1 is one of H and C1-C4 alkyl, and R2 is -CONH2, -CONHCH3, -CONHCH2CH3, -CON(CH3)2, -CON(CH2CH3)2, -CONHCH2OH, -CONHCH2CH2OH, -COO(CH2CH2O) a H, -COO(CH2) bOne of the functional groups PO3H, -COOM, -(C6H5)COOM, -SO3M and -(C6H5)SO3M, wherein a=1-40, b=1-12, and M is selected from one of H, Li+, Na+ and K+.

[0010] The general formula of the second monomer is CH2=CHCOOR3, wherein R3 is selected from a C2-C18 alkyl group or a C2-C18 alkyl group substituted by a hydroxyl group.

[0011] Among all monomers used to synthesize the water-based software, the molar proportion of all second monomers is greater than 50%.

[0012] By adopting the above technical solution, the above water-based soft glue is used together with a PAA (polyacrylic acid) water-based adhesive to prepare a hard carbon negative electrode sheet, which can significantly improve the stability and processing performance of the electrode sheet.

[0013] A preferred solution of the water-based soft glue for improving the softness and processing performance of the hard carbon negative electrode plate is that the water-based soft glue is obtained by a mixed polymerization reaction of a first monomer and a second monomer. The first monomer is acrylamide.

[0014] The second monomer is selected in the following manner: the homopolymer of the second monomer is a flexible adhesive with a glass transition temperature lower than -15° C. The second monomer is butyl acrylate or hydroxyethyl acrylate.

[0015] By adopting the above technical solution, the water-based soft gel prepared by this technology can significantly improve the softness and processing performance of the hard carbon negative electrode sheet.

[0016] A preferred solution for the aqueous soft gel for improving the softness and processing performance of the hard carbon negative electrode plate is that the aqueous latex is obtained by the following method: adding a surfactant and a protective colloid into water, then adding all the first monomers and all the second monomers, then adding an initiator, heating to 60 to 80° C. to carry out a polymerization reaction for 6 to 24 hours to obtain the aqueous soft gel.

[0017] By adopting the above technical scheme, the monomer forms small droplets and is dispersed in water to form an emulsion. The surfactant stabilizes the emulsion and maintains the orderly progress of the polymerization reaction to form latex particles. The protective colloid is adsorbed onto the surface of the generated latex particles to prevent the latex particles from agglomerating. The initiator forms free radicals after being heated to initiate the polymerization reaction. The initiator can be a persulfate, a peroxide, etc.

[0018] A preferred solution of the aqueous soft glue for improving the softness and processing performance of the hard carbon negative electrode plate is that the protective colloid is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose ether, hydroxymethyl cellulose ether, hydroxypropyl cellulose ether and polyvinyl pyrrolidone.

[0019] By adopting the above technical solution, the protective colloid is adsorbed onto the surface of the generated latex particles, preventing the latex particles from agglomerating and promoting the continuous reaction.

[0020] A preferred solution of the aqueous soft glue for improving the softness and processing performance of the hard carbon negative electrode sheet is that the surfactant is selected from one or more of nonionic surfactants and anionic surfactants.

[0021] By adopting the above technical solution, the nonionic surfactant absorbs a large amount of water through hydrogen bonding, thereby stabilizing the emulsion. The lipophilic end of the anionic surfactant absorbs the oil phase liquid, and the hydrophilic end has a negative charge, which makes the oil phase droplets repel each other and prevents the droplets from aggregating, thereby stabilizing the emulsion.

[0022] In the second aspect, the present application proposes a method for preparing a hard carbon negative electrode sheet and adopts the following technical solution.

[0023] A method for preparing a hard carbon negative electrode sheet, the method comprising: mixing a polyacrylic acid aqueous binder and water, dispersing them uniformly, adding conductive carbon black, dispersing them uniformly, then adding a hard carbon negative electrode material, dispersing them uniformly, obtaining a primary slurry, adjusting the viscosity of the primary slurry at 25° C. to between 3000 and 4000 mPa·s, then adding the above-mentioned aqueous soft glue, dispersing them uniformly, obtaining a secondary slurry. The secondary slurry is coated on a copper foil, dried, and cut to obtain the hard carbon negative electrode sheet.

[0024] In the above method, by mass, polyacrylic acid aqueous binder: conductive carbon black: hard carbon negative electrode material: aqueous soft gelatin = (2-3): (0.5-1.5): (94-97): 1.

[0025] By adopting the above technical solution, the polyacrylic acid water-based adhesive and the water-based soft adhesive are used together to achieve a significant improvement in the softness and processing performance of the hard carbon negative electrode sheet.

[0026] A preferred embodiment of the method for preparing the hard carbon negative electrode sheet is that the mass ratio of the total amount of the polyacrylic acid aqueous adhesive, the conductive carbon black, the hard carbon negative electrode material and the aqueous soft glue to water is 100:(100-150).

[0027] By adopting the above technical solution, the slurry after mixing the above materials has a suitable viscosity, is not easy to settle, and has a suitable density after drying, which significantly improves the softness and processing performance of the hard carbon negative electrode. Among them, the viscosity of the primary slurry can be achieved by adjusting its water content.

[0028] A preferred embodiment of the preparation method of the hard carbon negative electrode plate is as follows: take a polyacrylic acid aqueous binder and half of the water and mix them in a blender, disperse them at a speed of 250-350 rpm for 10-20 minutes, then add conductive carbon black, stir at a speed of 100-200 rpm for 5-15 minutes, and then stir at a high speed of 600-1000 rpm for 100-140 minutes. The speed is lowered to 250-300 rpm, half of the hard carbon negative electrode material is added, dispersed for 5-15 minutes, and the remaining half of the hard carbon negative electrode material and the remaining half of the water are added and dispersed for 5-15 minutes, and then stirred at a high speed of 600-1000 rpm for 100-140 minutes to obtain a primary slurry. The viscosity of the primary slurry is adjusted to between 3000 and 4000 mPa·s at 25°C by regulating the water content of the primary slurry. Add the water-based soft glue to the primary slurry, disperse at 450-550rpm for 20-40min, and filter with a 100-200 mesh filter to obtain a secondary slurry. Place the copper foil on a coating machine, evenly coat it with the secondary slurry, dry it, and finally cut it to obtain a hard carbon negative electrode sheet.

[0029] By adopting the above technical solution, each component is fully dispersed, and the flexibility and processing performance of the electrode are significantly improved.

[0030] On the third aspect, the present application also proposes a hard carbon negative electrode plate and adopts the following technical solution.

[0031] A hard carbon negative electrode sheet is prepared according to the above preparation method.

[0032] By adopting the above technical solution, the softness and processing performance of the electrode sheet are significantly improved, providing a new solution for the preparation of hard carbon negative electrode sheets for sodium ion batteries.

[0033] In summary, the water-based soft glue, hard carbon negative electrode sheet and preparation method thereof for improving the softness and processing performance of the hard carbon negative electrode sheet of the present application have the following beneficial effects: The present application provides a water-based soft glue, which can improve the softness and processing performance of the hard carbon negative electrode sheet by being used in combination with a PAA-type water-based adhesive, and solve the problems of the sheet being hard and brittle, easy to crack and drop. This technology is applicable to the preparation process of the hard carbon negative electrode sheet of the sodium ion battery, and has a significant application effect, especially in the scenario where the softness and processing performance of the sheet need to be improved.

[0034] The water-based soft glue prepared by the present application can significantly improve the softness and processing performance of the hard carbon negative electrode by introducing a specific proportion of soft monomers with a Tg lower than -15°C. Compared with soft glues such as SBR (styrene-butadiene rubber), PVAC (polyvinyl acetate), and VAE (ethylene-vinyl acetate copolymer), the hard carbon electrode prepared by the present application performs outstandingly in both the softness test and the needle rolling test, while maintaining a high electrode adhesion and cohesion. DETAILED DESCRIPTION

[0035] Example 1 This embodiment prepares a water-based soft glue.

[0036] The general formula of the first monomer is CH2=CR1R2. The first monomer used in this embodiment is acrylamide, that is, R1 is H and R2 is -CONH2.

[0037] The general formula of the second monomer is CH2=CHCOOR3. The second monomer used in this embodiment is butyl acrylate, that is, R3 is a C4 alkyl group.

[0038] The preparation method of water-based latex is as follows.

[0039] Take materials by mass, add 1 part of surfactant and 1 part of protective colloid to 100 parts of water, then add 30 parts of the first monomer and 50 parts of the second monomer, then add 0.1 parts of initiator, heat to 70°C for polymerization reaction for 10 hours, and obtain a water-based soft gel.

[0040] In the above preparation method, the surfactant is alkylphenol polyoxyethylene ether, the protective colloid is polyvinyl alcohol, and the initiator is ammonium persulfate.

[0041] Example 2 The method for preparing the hard carbon negative electrode sheet is as follows.

[0042] Take materials by mass, take 2 parts of polyacrylic acid aqueous adhesive and 60 parts of water and mix them in a blender, disperse them at 300 rpm for 15 minutes, then add 1 part of SP conductive carbon black, stir at 150 rpm for 10 minutes, and then stir at 800 rpm for 120 minutes; lower the speed to 300 rpm, add 48 parts of hard carbon negative electrode material, disperse for 10 minutes, then add 48 parts of hard carbon negative electrode material and 60 parts of water and disperse for 10 minutes, then stir at 800 rpm for 120 minutes to obtain a primary slurry; adjust the viscosity of the primary slurry to 3587 mPa·s at 25°C by regulating the water content of the primary slurry; add 1 part of the aqueous soft glue prepared in Example 1 to the primary slurry, disperse at 500 rpm for 30 minutes, and filter with a 150-mesh filter to obtain a secondary slurry.

[0043] Place the copper foil on the coating machine, evenly coat the secondary slurry, send it into a 100℃ environment and bake it until dry, cut it into 12.5cm×5cm specifications, and the single-sided density is 100-110g / m 2 Hard carbon negative electrode.

[0044] Test Example 1 Pole peeling force test method: Place the cut pole pieces in a 35% RH constant temperature room for 30 minutes. Place the two pole pieces together with the coating facing outward and the copper foil facing inward, and place them in an electric roller press to roll the pole pieces to a compaction density of 0.95g / cm 3 , and then place it for 30 minutes after rolling. During this period, select five 12.5cm×5cm stainless steel plates, stick double-sided tape of corresponding specifications on the stainless steel plates, and then stick the electrode on the double-sided tape with the coating facing down, and then stick a 2.5cm wide masking tape on the copper foil. The electrode steel plate is rolled back and forth by an electric rolling roller with a certain pressure (1kgf) for one week, and then an electronic stripping machine is used to test the adhesion of the electrode. The same method as above, only the electrode is stuck on the double-sided tape with the coating facing up to test the cohesion of the electrode.

[0045] The softness is tested using the softness tester IMT-RRD01*1.

[0046] Winding needle test: Use a cylindrical bending tester with model BEVS1603 to simulate the requirements of the winding process in battery cell preparation for the flexibility of the pole piece. The test result is the minimum diameter of the cylinder that can prevent the pole piece from cracking during the winding needle test.

[0047] The test results of the following items are shown in Table 1.

[0048] Table 1 Performance test of pole pieces prepared by four adhesive combinations In Table 1, the mass ratio of each adhesive combination is the former: the latter = 2:1. The first group of PAA + Example 1 is the electrode prepared in Example 2, and the methods for making the electrode in the other three groups of adhesive combinations are the same as in Example 2, that is, using SBR-Ryon, VAE, and PVAC of the same mass to replace the water-based soft glue prepared in Example 1, and finally preparing the electrode.

[0049] In Table 1, PAA is a polyacrylic acid water-based adhesive, Example 1 represents the water-based soft adhesive prepared in Example 1, SBR-Styrene-butadiene rubber prepared by Japan Styrene Corporation, VAE is a polymer emulsion formed by copolymerization of vinyl acetate and ethylene, and PVAC is a polyvinyl acetate emulsion adhesive.

[0050] As can be seen from Table 1, compared with soft gels such as SBR-Ryon, PVAC, and VAE, the hard carbon pole piece further prepared by the water-based soft gel prepared in this application performs outstandingly in both the softness test and the needle rolling test, while maintaining high pole piece adhesion and cohesion, providing a new solution for the preparation of hard carbon negative pole pieces for sodium ion batteries. This application introduces a specific proportion of soft monomers with a Tg lower than -15°C, and the water-based soft gel prepared in this application can significantly improve the softness and processing performance of the hard carbon negative pole piece.

[0051] The above are only some embodiments of the present application, and the protection scope of the present application is not limited to the above embodiments. For ordinary technicians in this technical field, some improvements and modifications without departing from the creative design of the present application should also fall within the protection scope of the present application.

Claims

1. A water-based soft glue for improving the softness and processing performance of a hard carbon negative electrode, characterized in that: The water-based soft glue is obtained by mixed polymerization of several first monomers and several second monomers; The first monomer has a general formula of CH2=CR1R2, wherein R1 is one of H and C1-C4 alkyl, and R2 is -CONH2, -CONHCH3, -CONHCH2CH3, -CON(CH3)2, -CON(CH2CH3)2, -CONHCH2OH, -CONHCH2CH2OH, -COO(CH2CH2O) a H, -COO(CH2) b One of PO3H, -COOM, -(C6H5)COOM, -SO3M and -(C6H5)SO3M functional groups, wherein a=1-40, b=1-12, and M is selected from one of H, Li+, Na+ and K+; The general formula of the second monomer is CH2=CHCOOR3, wherein R3 is selected from a C2-C18 alkyl group or a C2-C18 alkyl group substituted by a hydroxyl group; Among all monomers used to synthesize the aqueous software, the molar proportion of all second monomers is greater than 50%.

2. The water-based soft glue for improving the softness and processing performance of hard carbon negative electrode sheets according to claim 1, characterized in that: The water-based soft glue is obtained by a mixed polymerization reaction of a first monomer and a second monomer; the first monomer is acrylamide; The second monomer is selected in the following manner: the homopolymer of the second monomer is a flexible adhesive with a glass transition temperature lower than -15°C; the second monomer is butyl acrylate or hydroxyethyl acrylate.

3. The water-based soft glue for improving the softness and processing performance of hard carbon negative electrode sheets according to claim 1 or 2, characterized in that: The aqueous latex is obtained by the following method: adding a surfactant and a protective colloid into water, then adding all the first monomers and all the second monomers, then adding an initiator, heating to 60-80° C. to perform a polymerization reaction for 6-24 hours, and obtaining the aqueous soft glue.

4. The water-based soft glue for improving the softness and processing performance of hard carbon negative electrode sheets according to claim 3, characterized in that: The protective colloid is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose ether, hydroxymethyl cellulose ether, hydroxypropyl cellulose ether and polyvinyl pyrrolidone.

5. The water-based soft glue for improving the softness and processing performance of hard carbon negative electrode sheets according to claim 3, characterized in that: The surfactant is selected from one or more of nonionic surfactants and anionic surfactants.

6. A method for preparing a hard carbon negative electrode sheet, characterized in that: The preparation method comprises: Mix a polyacrylic acid aqueous binder and water, disperse them evenly, then add conductive carbon black, disperse them evenly, then add a hard carbon negative electrode material, disperse them evenly, and obtain a primary slurry. Adjust the viscosity of the primary slurry at 25° C. to between 3000 and 4000 mPa·s, then add the aqueous soft glue described in claims 1 to 5, disperse them evenly, and obtain a secondary slurry. Apply the secondary slurry on a copper foil, dry it, and cut it to obtain the hard carbon negative electrode sheet. In the above method, by mass, polyacrylic acid aqueous binder: conductive carbon black: hard carbon negative electrode material: aqueous soft gel = (2~3): (0.5~1.5): (94~97):

1.

7. The method for preparing a hard carbon negative electrode sheet according to claim 6, characterized in that: The mass ratio of the total amount of the polyacrylic acid aqueous adhesive, the conductive carbon black, the hard carbon negative electrode material and the aqueous soft glue to water is 100:(100-150).

8. The method for preparing a hard carbon negative electrode sheet according to claim 6 or 7, characterized in that: The preparation method is specifically: Take a polyacrylic acid aqueous binder and half of the water and mix them in a blender, disperse them at a speed of 250-350rpm for 10-20 minutes, then add conductive carbon black, stir at a speed of 100-200rpm for 5-15 minutes, and then stir at a high speed of 600-1000rpm for 100-140 minutes; adjust the speed down to 250-300rpm, add half of the hard carbon negative electrode material, disperse for 5-15 minutes, then add the remaining half of the hard carbon negative electrode material and the remaining half of the water and disperse for 5-15 minutes, then stir at a high speed of 600-1000rpm for 100-140 minutes to obtain a primary slurry; adjust the viscosity of the primary slurry to between 3000 and 4000mPa·s at 25°C by regulating the water content of the primary slurry; add the aqueous soft glue to the primary slurry, disperse it at 450-550rpm for 20-40min, and filter it with a 100-200 mesh filter to obtain a secondary slurry; Place the copper foil on a coating machine, evenly coat it with the secondary slurry, dry it, and finally cut it to obtain a hard carbon negative electrode sheet.

9. A hard carbon negative electrode plate, characterized in that: Prepared according to the preparation method according to any one of claims 6 to 8.

Citation Information

Patent Citations

  • Polyacrylate water-based adhesive for electrode materials of lithium ion battery, preparation method of adhesive and electrode plates of lithium ion battery

    CN104356979A

  • Anode aqueous binder of lithium ion battery and preparation method thereof

    CN105576284A

  • Lithium ion battery positive electrode aqueous adhesive and preparation method thereof

    CN106833448A

  • Lithium ion battery negative electrode aqueous adhesive and preparation method thereof

    CN107325225A

  • Water-based adhesive for secondary battery and preparation method of water-based adhesive

    CN116864691A

Cited By

  • Hard carbon negative electrode material based on surface modification of strong polar functional group and preparation method of hard carbon negative electrode material

    CN120511298A

  • A hard carbon anode material based on surface modification of strongly polar functional groups and its preparation method

    CN120511298B