Bio-based ultraviolet curing resin and preparation method thereof

By using bio-based raw materials such as acrylic pine acid and high-energy ball milling technology, micro-nano-scale maleic anhydride treated with high-energy ball milling technology, combined with ultraviolet curing methods, the problems of poor performance and complex preparation of bio-based ultraviolet curing resins are solved, and environmental protection and low cost are achieved The resin preparation improves curing speed and performance.

CN119039518APending Publication Date: 2024-11-29JIANGSU SHANGTAI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092947.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing bio-based ultraviolet curing resins have a gap in performance compared with petrochemical products, and the preparation process is complex and costly.

Method used

Using bio-based raw materials such as acrylic pine acid, micro-nano-scale maleic anhydride is treated through high-energy ball milling technology, combined with specific molecular weight control and addition of photoinitiators, crosslinking agents, UV stabilizers, catalysts, antioxidants and microbial antibacterial agents. Bio-based ultraviolet curing resin was prepared by equal volume method and ultraviolet curing method.

Benefits of technology

It improves the flowability, curing speed and performance of the resin, reduces production costs, and does not release harmful substances during use and waste, which is easy to biodegrade, and is in line with the trend of green and sustainable development.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a bio-based ultraviolet light-cured resin. The bio-based ultraviolet light-cured resin comprises the following components in percentage by weight: 25-30% of acrylpimaric acid, 10-30% of a cosolvent, 10-20% of a solvent, and the balance of a solvent. 5%-10% of diethylene glycol; 10%-15% of micro-nano maleic anhydride; 5-10% of acrylic acid; 10%-15% of maleopimaric acid acyl chloride; 5 to 10 percent of pentaerythritol; 5%-10% of dimethylolpropionic acid; 2-5% of a terminal propenyl group; 2-5% of a photoinitiator; 5-10% of a cross-linking agent; 2-5% of a UV stabilizer; 1-3% of a catalyst; 0.5-2% of an antioxidant; 0.5-2% of a microbial antibacterial agent; the molecular weight of the acrylpimaric acid is 300 to 500; the micro-nano-scale maleic anhydride is obtained by carrying out inorganic modification treatment on original maleic anhydride through a high-energy ball milling technology, and the particle size range is 10-50nm. The bio-based ultraviolet curing resin is derived from rosin, is simple in preparation process and excellent in performance, and has good environmental protection performance and wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation of ultraviolet light-curing resins, and more particularly to a bio-based ultraviolet light-curing resin and a preparation method thereof. Background Art

[0002] With the increasing awareness of environmental protection and the pursuit of sustainable development, traditional petroleum-based materials are gradually being replaced by bio-based materials. Bio-based materials not only come from renewable resources, but also have good biodegradability. UV-curable resins have been widely used in coatings, inks, adhesives and other fields due to their advantages such as fast curing, energy saving and low pollution. However, most of the UV-curable resins on the market are based on petrochemicals, which not only have limited resources, but also have environmental issues that are of concern.

[0003] In recent years, bio-based resins have received widespread attention due to their renewable, low-carbon and environmentally friendly characteristics. They are mainly derived from biomass, such as vegetable oil, starch, protein, etc., and have the advantages of wide sources and good renewability. However, there are still some bottlenecks in the application of bio-based resins in the field of UV curing. First, the performance of bio-based UV curing resins is still somewhat inferior to that of petrochemical products, such as wear resistance and chemical resistance. Secondly, the preparation process of bio-based UV curing resins is complicated and the cost is relatively high. Summary of the invention

[0004] In order to solve the problems existing in the prior art, a bio-based UV-curable resin and a preparation method thereof are provided. The specific scheme is as follows:

[0005] A bio-based UV-curable resin, the bio-based UV-curable resin comprising the following components in percentage by weight:

[0006] 25-30% of propylene pimaric acid; 5-10% of diethylene glycol; 10-15% of micro-nano maleic anhydride; 5-10% of acrylic acid; 10-15% of maleopimaric acid chloride; 5-10% of pentaerythritol; 5-10% of dimethylol propionic acid; 2-5% of terminal propylene group; 2-5% of photoinitiator; 5-10% of crosslinking agent; 2-5% of UV stabilizer; 1-3% of catalyst; 0.5-2% of antioxidant; 0.5-2% of microbial antibacterial agent; the molecular weight of the propylene pimaric acid is 300-500; the micro-nano maleic anhydride is obtained by inorganically modifying the original maleic anhydride through high-energy ball milling technology, and the particle size ranges from 10 to 50 nm.

[0007] Furthermore, the acrylpimaric acid is obtained by using toluene as a solvent, N-hydroxypropanesulfonamide and hydrogen peroxide as catalysts, and adopting an equal volume method to modify the free gene pimaric acid by free radical polymerization.

[0008] Furthermore, the photoinitiator is phenyl ketone, dihydropyrano[3,4-b]quinoline-1(2H)-one, and azobisisobutyrate.

[0009] Furthermore, the crosslinking agent is one or a mixture of triacrylate trimer, dimethacrylate or ursula nitrile acrylate.

[0010] Furthermore, the UV stabilizer is one or a mixture of the UV absorber 234 , the UV absorber 1130 and the ashing agent 770 .

[0011] Furthermore, the catalyst is one or a mixture of dimethyldiaminoethylene, tin o-toluenesulfonate and platinum black.

[0012] Furthermore, the antioxidant is BHT, BHA or one or a mixture of several of the antioxidants 1010.

[0013] Furthermore, the microbial antibacterial agent is one or a mixture of nano silver, aspergillus or nano zinc.

[0014] A method for preparing a bio-based ultraviolet curable resin comprises the following steps:

[0015] S1: mixing acrylpimaric acid, diethylene glycol, micro-nano maleic anhydride, acrylic acid, maleopimaric acid chloride, pentaerythritol, dimethylol propionic acid and terminal propylene group according to the percentages, stirring at a rate of 300 RPM for 30 minutes in a stirrer to obtain a uniform raw material mixture;

[0016] S2: adding a photoinitiator to the raw material mixture, and continuing to stir at a speed of 300 RPM for 30 minutes to obtain a mixed solution containing a photoinitiator;

[0017] S3: adding a crosslinking agent, a UV stabilizer, a catalyst antioxidant, and a microbial antibacterial agent to the mixed solution containing the photoinitiator in the above-mentioned proportions, and continuing to stir at a speed of 300 RPM for 60 minutes to obtain a completely mixed resin solution;

[0018] S4: Finally, pour the above resin solution into a pre-cleaned and dried metal or plastic mold and place it under ultraviolet light with a wavelength of 365nm and a light intensity of 1000mW / cm 2 The light exposure time is 5 to 20 minutes to fully cure it, and then it is naturally cooled at room temperature and demolded to obtain a bio-based UV-curable resin.

[0019] Beneficial effects:

[0020] The present invention provides a bio-based UV-curable resin and a preparation method thereof, which has the following advantages:

[0021] (1) The bio-based UV-curable resin of the present invention is mainly composed of bio-based raw materials such as acrylpimaric acid, which are derived from rosin. The raw materials are widely available and are more environmentally friendly than petrochemical products, which is in line with the current trend of green and sustainable development.

[0022] (2) The molecular weight of acrylpimaric acid is controlled within the range of 300 to 500. This specific molecular weight range enables the resin to have good fluidity and curing properties, thereby improving production efficiency and reducing production costs while ensuring product performance.

[0023] (3) Adding micro-nano-scale maleic anhydride, treating the maleic anhydride with high-energy ball milling technology, and controlling the particle size within the range of 10 to 50 nm, so that the dispersibility and activity of maleic anhydride in the resin are significantly improved, thereby improving the curing speed of the resin and the performance of the final product.

[0024] (4) The bio-based UV-curable resin of the present invention does not release any harmful substances during use and is easily biodegradable after being discarded, with little impact on the environment. DETAILED DESCRIPTION

[0025] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0026] Embodiment 1:

[0027] Step 1: Take 300 g of acrylpimaric acid with a molecular weight of 400, put it into a toluene solvent, add N-hydroxypropanesulfonamide and hydrogen peroxide as catalysts, and perform free radical polymerization modification according to the equal volume method to obtain modified acrylpimaric acid.

[0028] Step 2: Take the obtained modified propylene pimaric acid, diethylene glycol 100g, micro-nano maleic anhydride 150g (the original maleic anhydride is inorganically modified by high-energy ball milling technology, and the particle size is 30nm), acrylic acid 100g, maleopimaric acid chloride 150g, pentaerythritol 100g, dihydroxymethylpropionic acid 100g, and terminal propylene group 50g.

[0029] Step 3: Place the above components into a reactor, add 20g of photoinitiator (a mixture of phenyl ketone, dihydropyrano[3,4-b]quinoline-1(2H)-one, and azobisisobutyrate), 100g of crosslinker (a mixture of triacrylate trimer, dimethacrylate and ursulazolyl acrylate), 50g of UV stabilizer (a mixture of UV absorber 234, UV absorber 1130 and ashing agent 770), 30g of catalyst (a mixture of dimethyldiaminoethylene, tin o-toluenesulfonate and platinum black), 20g of antioxidant (BHT), and 20g of microbial antibacterial agent.

[0030] Step 4: Under the action of a stirrer, the mixture in the reaction kettle is stirred evenly, and then cured under ultraviolet light to obtain the bio-based ultraviolet curing resin.

[0031] Embodiment 2:

[0032] Step 1: 280 g of acrylpimaric acid with a molecular weight of 350 is taken, placed in a toluene solvent, N-hydroxypropanesulfonamide and hydrogen peroxide are added as catalysts, and free radical polymerization is performed according to an equal volume method to obtain modified acrylpimaric acid;

[0033] Step 2: the obtained modified propylene pimaric acid, diethylene glycol 90g, micro-nano maleic anhydride 140g (the original maleic anhydride is inorganically modified by high-energy ball milling technology, and the particle size is 40nm), acrylic acid 90g, maleopimaric acid chloride 140g, pentaerythritol 90g, dimethylol propionic acid 90g, terminal propylene group 45g;

[0034] Step 3: Put the above components into a reactor, add 18g of photoinitiator (a mixture of phenyl ketone, dihydropyrano[3,4-b]quinoline-1(2H)-one, and azobisisobutyrate), 90g of crosslinker (a mixture of triacrylate trimer, dimethacrylate and ursulpyrocyanate), 45g of UV stabilizer (a mixture of ultraviolet absorber 234, ultraviolet absorber 1130 and ashing agent 770), 27g of catalyst (a mixture of dimethyldiaminoethylene, tin o-toluenesulfonate and platinum black), 18g of antioxidant (BHT), and 18g of microbial antibacterial agent;

[0035] Step 4: Under the action of a stirrer, the mixture in the reaction kettle is stirred evenly, and then cured under ultraviolet light to obtain the bio-based ultraviolet curing resin.

[0036] Embodiment 3:

[0037] Step 1: Take 260 g of acrylpimaric acid with a molecular weight of 450, put it into a toluene solvent, add N-hydroxypropanesulfonamide and hydrogen peroxide as catalysts, and perform free radical polymerization modification according to the equal volume method to obtain modified acrylpimaric acid.

[0038] Step 2: The obtained modified propylene pimaric acid, diethylene glycol 80g, micro-nano maleic anhydride 130g (the original maleic anhydride is inorganically modified by high-energy ball milling technology, and the particle size is 35nm), acrylic acid 80g, maleopimaric acid chloride 130g, pentaerythritol 80g, dihydroxymethylpropionic acid 80g, and terminal propylene group 40g.

[0039] Step 3: Place the above components into a reactor, add 16g of photoinitiator (a mixture of phenyl ketone, dihydropyrano[3,4-b]quinoline-1(2H)-one, and azobisisobutyrate), 80g of crosslinker (a mixture of triacrylate trimer, dimethacrylate and ursulazolyl acrylate), 40g of UV stabilizer (a mixture of UV absorber 234, UV absorber 1130 and ashing agent 770), 24g of catalyst (a mixture of dimethyldiaminoethylene, tin o-toluenesulfonate and platinum black), 16g of antioxidant (BHT), and 16g of microbial antibacterial agent.

[0040] Step 4: Under the action of a stirrer, the mixture in the reaction kettle is stirred evenly, and then cured under ultraviolet light to obtain the bio-based ultraviolet curing resin.

[0041] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A bio-based UV-curable resin, characterized in that: The bio-based UV-curable resin comprises the following components in percentage by weight: 25-30% of propylene pimaric acid; 5-10% of diethylene glycol; 10-15% of micro-nano maleic anhydride; 5-10% of acrylic acid; 10-15% of maleopimaric acid chloride; 5-10% of pentaerythritol; 5-10% of dimethylol propionic acid; 2-5% of terminal propylene group; 2-5% of photoinitiator; 5-10% of crosslinking agent; 2-5% of UV stabilizer; 1-3% of catalyst; 0.5-2% of antioxidant; 0.5-2% of microbial antibacterial agent; the molecular weight of the propylene pimaric acid is 300-500; the micro-nano maleic anhydride is obtained by inorganically modifying the original maleic anhydride through high-energy ball milling technology, and the particle size ranges from 10 to 50 nm.

2. The bio-based UV-curable resin according to claim 1, characterized in that: The acrylpimaric acid is obtained by using toluene as a solvent, N-hydroxypropanesulfonamide and hydrogen peroxide as catalysts, and adopting an equal volume method to perform free radical polymerization modification on free gene pimaric acid.

3. The bio-based UV-curable resin according to claim 1, characterized in that: The photoinitiator is phenyl ketone, dihydropyrano[3,4-b]quinoline-1(2H)-one, and azobisisobutyrate.

4. The bio-based UV-curable resin according to claim 1, characterized in that: The crosslinking agent is one or a mixture of triacrylate trimer, dimethacrylate or ursula nitrile acrylate.

5. The bio-based UV-curable resin according to claim 1, characterized in that: The UV stabilizer is one of the ultraviolet absorber 234, the ultraviolet absorber 1130 and the ashing agent 770 or a mixture of several of them.

6. The bio-based UV-curable resin according to claim 1, characterized in that: The catalyst is one or a mixture of dimethyldiaminoethylene, tin o-toluenesulfonate and platinum black.

7. The bio-based UV-curable resin according to claim 1, characterized in that: The antioxidant is BHT, BHA or one or a mixture of several of the antioxidants 1010.

8. The bio-based UV-curable resin according to claim 1, characterized in that: The microbial antibacterial agent is one or a mixture of nano silver, aspergillus or nano zinc.

9. A method for preparing a bio-based UV-curable resin according to claims 1 to 8, characterized in that: The following steps are involved: S1: mixing acrylpimaric acid, diethylene glycol, micro-nano maleic anhydride, acrylic acid, maleopimaric acid chloride, pentaerythritol, dimethylol propionic acid and terminal propylene group according to the percentages, stirring at a rate of 300 RPM for 30 minutes in a stirrer to obtain a uniform raw material mixture; S2: adding a photoinitiator to the raw material mixture, and continuing to stir at a speed of 300 RPM for 30 minutes to obtain a mixed solution containing a photoinitiator; S3: adding a crosslinking agent, a UV stabilizer, a catalyst antioxidant, and a microbial antibacterial agent to the mixed solution containing the photoinitiator in the above-mentioned proportions, and continuing to stir at a speed of 300 RPM for 60 minutes to obtain a completely mixed resin solution; S4: Finally, pour the above resin solution into a pre-cleaned and dried metal or plastic mold and place it under ultraviolet light with a wavelength of 365nm and a light intensity of 1000mW / cm 2 The light exposure time is 5 to 20 minutes to fully cure it, and then it is naturally cooled at room temperature and demolded to obtain a bio-based UV-curable resin.