Photoelectric dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional forming

By introducing olefin double bond-like ionic liquids and nanospheres into photonic crystal hydrogels and using DLP three-dimensional molding technology to form an interconnected network, the assembly limitations and response sensitivity issues of photonic crystal hydrogels have been solved. This has enabled the development of a rapid-molding and highly sensitive optoelectronic dual-mode hydrogel material suitable for smart wearables and biosensors.

CN119039622APending Publication Date: 2024-11-29ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411162367.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing photonic crystal hydrogels face limitations in nanosphere or assembly, response mechanisms, the isolation of photonic crystal materials, limitations in multiple responses and response sensitivity, and the complexity of preparation methods.

Method used

Using olefin double bond ionic liquids as functional monomers for hydrogels, and through DLP three-dimensional molding technology, their ionic properties and hydrophilicity are utilized to form an interconnected network after polymerization and cross-linking, realizing the self-assembly of low solid content nanospheres and forming a locally high solid content liquid photonic crystal structure. Combining the hydrogel polymerization network and nanosphere crystal clusters, a dual-mode "photoelectric" response is achieved.

Benefits of technology

Rapid prototyping and high-sensitivity response of photoelectric dual-mode responsive hydrogels have been achieved. These hydrogels possess excellent conductivity and superabsorbency, making them suitable for applications such as responsive biomimetic skin, smart wearable devices, and biosensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006805930000031
    Figure BDA0005006805930000031
  • Figure BDA0005006805930000041
    Figure BDA0005006805930000041
  • Figure BDA0005006805930000042
    Figure BDA0005006805930000042
Patent Text Reader

Abstract

The invention discloses a photoelectric dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional forming, and in the DLP three-dimensional forming process, an alkene double bond ionic liquid and a cross-linking agent are initiated by a photoinitiator with a specific structure to be subjected to in-situ polymerization and cross-linking to form an ionic polymer cross-linked network structure with a super water absorption characteristic. On one hand, the cross-linked network structure of the ionic polymer can induce directional migration of water molecules in a photonic crystal hydrogel working solution and induce self-assembly of ionic nano-microspheres to form a liquid photonic crystal cluster; and on the other hand, the hydrogel material is endowed with excellent conductivity by virtue of the intercommunicated and interconnected ionic polymer cross-linked network structure and the ionic liquid photonic crystal cluster. The photocuring three-dimensional forming hydrogel material can realize high-sensitivity response to changes such as stretching, compression and swelling under'photoelectric 'dual modes, and has wide application prospects in the fields of responsive bionic skin, intelligent wearable devices, biosensors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogel materials, and in particular relates to an optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding. Background Art

[0002] Responsive photonic crystal hydrogel materials have unique optical properties and stimulus response capabilities, and can achieve precise regulation of optical, electrical and other properties under external stimuli (such as temperature, pH value, mechanical stretching, etc.), playing an important role in smart wearables, sensors, optical communications and biosensors. However, responsive photonic crystal hydrogels still face great challenges in terms of precise control of periodic structures, design and synthesis of polymer network structures, multiple responses and response sensitivity, and mechanical and chemical stability.

[0003] CN107236085B discloses a method for rapidly preparing a large-area stretched photonic crystal hydrogel double-layer film. The method uses 50wt% high-concentration composite microspheres as the photonic crystal hydrogel assembly material and uses light-initiated crosslinking and curing. However, due to the characteristics of the nano-microsphere polymer, the high-concentration dispersion will affect the degree and efficiency of photocrosslinking.

[0004] CN116903780A discloses a photonic crystal hydrogel sensor and its preparation method and application. The method uses a photonic crystal assembled by PSt@SiO2 as a template, removes the SiO2 shell after filling the hydrogel, and forms a special opal and inverse opal composite structure. The method not only has high requirements on the nano-microsphere structure, but also easily damages the inverse protein structure when etching the SiO2 shell template, affecting the structural color effect.

[0005] CN110632060A discloses a Zika virus detection kit based on photonic crystal enhanced electrochemical luminescence and its preparation method. The method uses a photonic crystal substrate as an electrical signal amplifier and a Ru(bpy)3 2+ -COOH labeling as a sandwich immunosensor, but it only uses photonic crystals as electrical signal amplifiers, and fails to reflect the photonic crystal structural color response and other multiple response characteristics. CN115806715A discloses a photonic crystal 3D printing precursor, a photonic crystal and a preparation method thereof, characterized in that a polymer shell is coated on the surface of silica nanoparticles, so that the surface energy of the silica core-shell particles is reduced, and there is a tendency to self-assemble in the system, and the silica core-shell particles are mixed with pre-crosslinked gel to obtain a photonic crystal 3D printing precursor with bright structural color. This method puts forward special requirements on the hardness and surface properties of nano-microspheres, and organic soft microspheres are excluded, which limits the selection of microsphere materials for this method.

[0006] Similarly, a high-strength photonic crystal hydrogel and its preparation method and application disclosed in CN110041464A utilizes the swelling of soft polymer colloidal nanospheres by oil-soluble monomers and uses the nanospheres as crosslinking points of the hydrogel polymer network to prepare a photonic crystal hydrogel with stretch responsiveness. This method expands the selection range of nanospheres and monomers to a certain extent, but it still does not have wide applicability.

[0007] CN117624459A discloses a 3D printing precursor liquid and a preparation method thereof, as well as a three-dimensional photonic crystal and a preparation method thereof, characterized in that the 3D printing precursor liquid contains a monomer, a cross-linking agent, a photoinitiator, colloidal particles and a solvent, wherein hydrogen bonds can be formed between the monomer and the colloidal particles, and the presence of hydrogen bonds ensures the uniform distribution of the colloidal particles in the polymer skeleton. This method also needs to be washed to prepare an inverse opal structure and / or the solvent volatilizes to dry and assemble during color development to achieve a three-dimensional structure of structural color. Summary of the invention

[0008] The present invention aims to provide a photoelectric dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding, aiming at the defects in the prior art, solving the problems of the limitations of nano-microspheres or assemblies in the existing methods in the field of existing photonic crystal hydrogels, the isolation of the response mechanism and the photonic crystal materials, the limitations of multiple responses and response sensitivity, the complexity of the preparation method, etc. The present invention uses olefin double-bond ionic liquids as hydrogel functional monomers, on the one hand, utilizing its ionic properties to form an interconnected network after polymerization and cross-linking to achieve excellent conductivity; on the other hand, utilizing its hydrophilicity, after polymerization and cross-linking, it can achieve super water absorption properties, induce the self-assembly of low-solid nano-microspheres within a limited range, and form a liquid photonic crystal structural color effect with overall low solid content and local high solid content. In addition, based on the topological structure of the hydrogel polymerization cross-linking network and the nano-microsphere crystal cluster, the "photoelectric" dual-mode response of the hydrogel material under the action of physical mechanical force, swelling, etc. is achieved.

[0009] In order to solve the above technical problems, the following technical solutions are adopted:

[0010] An optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding, characterized in that: the hydrogel material precursor liquid is made of the following raw materials in weight percentage:

[0011] 5-16 wt% olefin-functionalized ionic liquid;

[0012] 0.8-6 wt% ionic crosslinking agent;

[0013] 0.05-16wt% salt photoinitiator;

[0014] 1-25wt% nano-microsphere dispersion;

[0015] 0.01-0.30wt% stray light absorber.

[0016] Preferably, the alkenyl functionalized ionic liquid is selected from one or two or more of the following, and the following are all of the same charge:

[0017]

[0018] After optimization, X - is an anion selected from the following:

[0019]

[0020] Preferably, the ionic crosslinking agent is consistent with the charge type of the selected alkenyl functionalized ionic liquid monomer, and is selected from one or two or more of the following:

[0021]

[0022] Preferably, the salt photoinitiator is selected from one of phenyl (2,4,6-trimethylbenzoyl) phosphonic acid lithium salt, phenyl (2,4,6-trimethylbenzoyl) phosphonic acid sodium salt, phenyl (2,4,6-trimethylbenzoyl) phosphonic acid magnesium salt, phenyl bis (2,4,6-trimethylbenzoyl) phosphonic acid sodium salt, phenyl bis (2,4,6-trimethylbenzoyl) phosphonic acid lithium salt, tris (4,4-dicarboxy bipyridine) ruthenium chloride, (4,4-dicarboxy bipyridine) ruthenium chloride, (2,2'-bipyridine) bis [2- (2,4-difluorophenyl) pyridine], tris (2,2'-bipyridine) ruthenium (II) chloride, tris (2,2'-bipyridine) dichloride, dihydroxyacetone phosphate dilithium salt, and 5- (-thio) adenosine triphosphate tetralithium salt.

[0023] Preferably, the nanosphere dispersion is selected from any one of a nanosphere dispersion containing cationic groups on the surface, a nanosphere dispersion containing anionic groups on the surface, an inorganic nanosphere dispersion, and an inorganic metal-coated nanosphere dispersion.

[0024] Preferably, the nanosphere dispersion containing cationic groups on the surface is selected from any one of poly(styrene-chitosan) (P(St-CHS)) nanospheres, poly(styrene-N-isopropylacrylamide) (P(St-NIPAM)) nanospheres, polypyrrole (PPy) nanospheres, polypyridine polystyrene@poly N-isopropylacrylamide (PSt@PNIPAM) nanospheres, poly(methacrylate-chitosan) (P(MMA-CHS)) nanospheres, poly(methacrylate-N-isopropylacrylamide) (P(MMA-NIPAM)) nanospheres, and polymethacrylate@poly N-isopropylacrylamide (PMMA@PNIPAM) nanospheres;

[0025] The nanosphere dispersion containing anionic groups on the surface is selected from any one of poly(sodium p-styrene sulfonate) (PSSS) nanospheres, polystyrene@polyacrylic acid (PSt@PAA) nanospheres, polystyrene@poly(methacrylate-acrylic acid) (PSt@P(MMA-AA)) nanospheres, poly(styrene-methyl methacrylate-acrylic acid) (P(St-MMA-AA)) nanosphere dispersion, poly(styrene-methyl methacrylate-methacrylic acid) (P(St-MMA-MAA)) nanospheres, and polyacrylic acid-b-polystyrene (PAA-b-PSt) nanospheres.

[0026] After optimization, the inorganic nano-microsphere dispersion is selected from any one of ferroferric oxide (Fe3O4) nano-microspheres and copper oxide (CuO) nano-microspheres;

[0027] The inorganic metal-coated nano-microsphere dispersion is selected from any one of nano-microspheres coated with gold (Au) on the surface and nano-microspheres coated with nickel (Ni) on the surface.

[0028] After optimization, the solid content of the nano-microsphere dispersion is 1% to 25%; the diameter of the nano-microsphere is 130 to 340 nm, and the monodispersity index is less than 0.08.

[0029] After optimization, the precursor liquid of the hydrogel material is placed in the liquid storage tank of the DLP printing equipment; the DLP printing parameters are adjusted: the layer thickness is set to 0.05-0.15 mm, the initial exposure time is 40-70 s, the printing exposure time is 4-9 s, the light-off delay time is 5-16 s, the printing rise height is 5-6 mm, the motor speed is 0.1-2 mm / s, and irradiation cross-linking is performed under any one of the UV-LEDs with a main wavelength of 365, 395, and 405 nm to obtain an optoelectronic dual-mode responsive photonic crystal hydrogel material with a customized three-dimensional structure and structural color effect.

[0030] The above technical solution has the following beneficial effects:

[0031] 1. The present invention innovatively proposes a low-viscosity hydrogel precursor suitable for digital light processing (DLP), and forms a strategy of in-situ color-developing "photoelectric" dual-mode responsive photonic crystal hydrogel through layer-by-layer solidification. A kind of olefin functionalized ionic liquid is also designed and prepared as a "photoelectric" dual-mode responsive hydrogel monomer and liquid photonic crystal inducer, which not only meets the low viscosity requirement of DLP printing working fluid, but also in the DLP three-dimensional molding process, the photoinitiator generates active free radicals under the irradiation of light of a specific wavelength, which triggers the in-situ polymerization and crosslinking of olefin double bond ionic liquids and ionic crosslinkers to form an "ionic polymer" crosslinked network structure with super water absorption properties. On the one hand, the "ionic polymer" crosslinked network structure can induce the directional migration of water molecules in the photonic crystal hydrogel working fluid, and induce the self-assembly of ionic nano-microspheres to form liquid photonic crystal clusters; on the other hand, the interconnected "ionic polymer" coach network structure supplemented by the structure of ionic liquid photonic crystal clusters gives the hydrogel material excellent conductivity. The prepared photocurable three-dimensional hydrogel material can achieve highly sensitive response to changes such as stretching, compression and swelling under "photoelectric" dual modes, and has broad application prospects in the fields of responsive bionic skin, smart wearable devices and biosensors.

[0032] 2. There are great differences in the implementation principles of structural color hydrogels and conductive hydrogels. The present invention cleverly uses functional ionic liquids of olefin double bonds with special structures, and realizes the three-dimensional molding of "photoelectric" dual-mode response hydrogels through in-situ polymerization and cross-linking of the "ionic polymer" network structure under DLP light irradiation. On the one hand, the multi-ion structure in the ionic liquid polymer network has extremely strong water absorption, which can induce the directional migration of water around the nano-microspheres, and under the action of the electrostatic repulsion between the polymer network and the nano-microsphere clusters, it induces the self-assembly of low-solid content nano-microspheres to form pre-crystallized clusters and liquid photonic crystal structures; on the other hand, the surface ionic photonic crystal nano-microsphere clusters can cooperate with the ionic liquid ionic polymer network structure to further reduce the internal resistance of the hydrogel material and improve the conductive performance and response sensitivity.

[0033] 3. The present invention utilizes the low viscosity characteristics of olefin double bond ionic liquids and low solid content nano-microsphere dispersions, and uses a DLP three-dimensional molding system under a projection light curing method to achieve rapid molding and structural customization of "photoelectric" dual-mode responsive hydrogel materials;

[0034] 4. The topological network structure formed by the ionic liquid polymer network structure and the local high-concentration nano-microsphere crystal clusters gives the conductive structural color hydrogel material "photoelectric" dual-mode response and high-sensitivity response under mechanical stretching, swelling, etc., and has broad application prospects in the fields of responsive bionic skin, smart wearable devices and biosensors. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0036] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0037] Example 1

[0038] (1) Preparation of photoelectric dual-mode responsive photonic crystal hydrogel working solution (i.e., hydrogel precursor solution) for DLP three-dimensional molding:

[0039] 20g of 1-allyl-3-methylimidazolium tetrafluoroborate was added to 100g of 5% PPy nanosphere dispersion, and the mixture was stirred evenly. The system color was not obvious. 0.05wt% of stray light absorber, 1g of ionic crosslinker 3-(N,N-diallyl-N-methylammonium) propanesulfonate and 1g of photoinitiator 5-(-thio) adenosine triphosphate tetralithium salt were added to prepare a DLP three-dimensional photocurable in-situ color-developing photonic crystal hydrogel working solution, which was stored away from light for later use.

[0040] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0041] The photocurable in-situ color-developing photonic crystal hydrogel working solution prepared in step (1) was placed in the liquid storage tank of the DLP printing device, and the layer thickness was adjusted to 0.02 mm, the printing exposure was 5 s, the light-off delay was 5 s, the printing rise height was 5 mm, and the motor speed was 0.6 mm / s. A 365 nm light source was used, and the printing device was turned on. After printing was completed, a DLP three-dimensionally molded photonic crystal hydrogel was obtained.

[0042] Example 2

[0043] (1) Preparation of photonic dual-mode responsive photonic crystal hydrogel working fluid for DLP three-dimensional molding:

[0044] 14 g of 1-allyl-3-ethylimidazolium bis(trifluoromethanesulfonyl)imide salt was added to 100 g of 1% PSSS nanosphere dispersion, and the mixture was stirred evenly. The system had no structural color. 0.04 wt% of stray light absorber, 3 g of ionic crosslinker 3,3'-(butane-1,4-diyl)bis(1-vinyl-3-imidazolium)imide salt and 3 g of photoinitiator phenyl(2,4,6-trimethylbenzoyl)phosphonic acid lithium salt were added to prepare a DLP three-dimensionally formed light-cured in-situ color-developing photonic crystal hydrogel working solution, which was stored away from light for later use.

[0045] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0046] The photocurable in-situ color-developing structured chromogenic hydrogel working solution prepared in step (1) is placed in the liquid storage tank of the DLP printing device, and the layer thickness is adjusted to 0.03 mm, the printing exposure is 5 s, the light-off delay is 6 s, the printing rise height is 4 mm, and the motor speed is 0.6 mm / s. A 395 nm light source is used, and the printing device is turned on. After printing is completed, a DLP three-dimensionally formed photonic crystal hydrogel is obtained.

[0047] Example 3

[0048] (1) Preparation of photonic dual-mode responsive photonic crystal hydrogel working fluid for DLP three-dimensional molding:

[0049] 30g of N-allyl-N-methylpiperidinium hexafluorophosphate was added to 100g of 10% PAA-b-PSt nanosphere dispersion, and the mixture was stirred evenly until the system color was not obvious. 0.1wt% of stray light absorber, 1.8g of ionic crosslinker 1-allyl-3-vinylimidazole hexafluorophosphate and 2.5g of photoinitiator dihydroxyacetone phosphate dilithium salt were added to prepare a DLP three-dimensional photocurable in-situ color-developing photonic crystal hydrogel working solution, which was stored away from light for later use.

[0050] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0051] The photocurable in-situ color-developing photonic crystal hydrogel working solution prepared in step (1) was placed in the liquid storage tank of the DLP printing device, and the layer thickness was adjusted to 0.03 mm, the printing exposure was 6 s, the light-off delay was 9 s, the printing rise height was 5 mm, and the motor speed was 0.3 mm / s. A 395 nm light source was used, and the printing device was turned on. After printing was completed, a DLP three-dimensionally molded photonic crystal hydrogel was obtained.

[0052] Example 4

[0053] (1) Preparation of photonic dual-mode responsive photonic crystal hydrogel working fluid for DLP three-dimensional molding:

[0054] 26g of 1-vinyl-3-methylimidazolium bis(fluorosulfonyl)imide salt and 4g of 1-allyl-3-hexylimidazolium chloride salt were added to 100g of 16% PSt@Au nanosphere dispersion, and the mixture was stirred evenly. The system color was not obvious. 0.12wt% of stray light absorber, 1.8g of ionic crosslinker 3-(N,N-diallyl-N-methylammonium) propanesulfonate and 1.7g of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphonic acid lithium salt were added to prepare a DLP three-dimensional photocurable in-situ color-developing photonic crystal hydrogel working solution, which was stored away from light for later use.

[0055] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0056] The photocurable in-situ color-developing photonic crystal hydrogel working solution prepared in step (1) was placed in the liquid storage tank of the DLP printing device, and the layer thickness was adjusted to 0.02 mm, the printing exposure was 5 s, the light-off delay was 13 s, the printing rise height was 5 mm, and the motor speed was 0.6 mm / s. A 365 nm light source was used, and the printing device was turned on. After printing, a DLP three-dimensionally molded photonic crystal hydrogel was obtained.

[0057] Embodiment 5:

[0058] (1) Preparation of photonic dual-mode responsive photonic crystal hydrogel working fluid for DLP three-dimensional molding:

[0059] 16g of sodium p-styrene sulfonate and 6g of N-allyl-N-methylpiperidinium bromide are added to 100g of 5% CuO nanosphere dispersion, and the mixture is stirred evenly. The system color is not obvious. 0.05wt% of stray light absorber, 0.9g of ionic crosslinker 3,3'-(butane-1,4-diyl)bis(1-vinyl-3-imidazolium)bis(trifluoromethanesulfonyl)imide salt and 3.4g of photoinitiator phenyl(2,4,6-trimethylbenzoyl)phosphonic acid sodium salt are added to prepare a DLP three-dimensional photocurable in-situ color-developing photonic crystal hydrogel working solution, which is stored away from light for later use.

[0060] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0061] The photocurable in-situ color-developing photonic crystal hydrogel working solution prepared in step (1) was placed in the liquid storage tank of the DLP printing device, and the layer thickness was adjusted to 0.03 mm, the printing exposure was 6 s, the light-off delay was 8 s, the printing rise height was 5 mm, and the motor speed was 0.4 mm / s. A 405 nm light source was used, and the printing device was turned on. After printing was completed, a DLP three-dimensionally molded photonic crystal hydrogel was obtained.

[0062] Embodiment 6:

[0063] (1) Preparation of photonic dual-mode responsive photonic crystal hydrogel working fluid for DLP three-dimensional molding:

[0064] 24g of N-allyl-N-methylpiperidinium bis(trifluoromethanesulfonyl)imide salt and 7g of sodium p-styrenesulfonate were added to 100g of 25% PMMA@Ni nanosphere dispersion, and the mixture was stirred evenly. The system color was not obvious. 0.05wt% of stray light absorber, 0.9g of ionic crosslinker 1-allyl-3-vinyl imidazole hexafluorophosphate and 3.4g of photoinitiator tris(4,4-dicarboxyl bipyridyl) ruthenium chloride were added to prepare a DLP three-dimensional photocurable in-situ color-developing photonic crystal hydrogel working solution, which was stored away from light for later use.

[0065] (2) DLP three-dimensional molding of photocurable in-situ color-developing photonic crystal hydrogels:

[0066] The photocurable in-situ color-developing photonic crystal hydrogel working solution prepared in step (1) was placed in the liquid storage tank of the DLP printing device, and the layer thickness was adjusted to 0.03 mm, the printing exposure was 6 s, the light-off delay was 15 s, the printing rise height was 5 mm, and the motor speed was 0.4 mm / s. A 405 nm light source was used, and the printing device was turned on. After printing was completed, a DLP three-dimensionally molded photonic crystal hydrogel was obtained.

[0067] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.

Claims

1. An optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding, characterized by: The hydrogel material precursor solution is made of the following raw materials in percentage by weight: 5-16 wt% olefin-functionalized ionic liquid; 0.8-6 wt% ionic crosslinking agent; 0.05-16wt% salt photoinitiator; 1-25wt% nano-microsphere dispersion; 0.01-0.30wt% stray light absorber.

2. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: The alkenyl functionalized ionic liquid is selected from one or two or more of the following, and the following are all of the same charge:

3. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 2, characterized in that: X - is an anion selected from the following:

4. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: The ionic crosslinking agent is consistent with the charge type of the selected alkenyl functionalized ionic liquid monomer, and is selected from one or two or more of the following:

5. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: The salt photoinitiator is selected from one of phenyl (2,4,6-trimethylbenzoyl) phosphonic acid lithium salt, phenyl (2,4,6-trimethylbenzoyl) phosphonic acid sodium salt, phenyl (2,4,6-trimethylbenzoyl) phosphonic acid magnesium salt, phenyl bis (2,4,6-trimethylbenzoyl) phosphonic acid sodium salt, phenyl bis (2,4,6-trimethylbenzoyl) phosphonic acid lithium salt, tri (4,4-dicarboxyl bipyridine) ruthenium chloride, (4,4-dicarboxyl bipyridine) ruthenium chloride, (2,2'-bipyridine) bis [2- (2,4-difluorophenyl) pyridine], tri (2,2'-bipyridine) ruthenium (II) chloride, tri (2,2'-bipyridine) dichloride, dihydroxyacetone phosphate dilithium salt, 5- (-thio) adenosine triphosphate tetralithium salt.

6. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: The nanosphere dispersion is selected from any one of a nanosphere dispersion containing cationic groups on the surface, a nanosphere dispersion containing anionic groups on the surface, an inorganic nanosphere dispersion, and an inorganic metal-wrapped nanosphere dispersion.

7. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 6, characterized in that: The nanosphere dispersion containing cationic groups on the surface is selected from any one of poly(styrene-chitosan) nanospheres, poly(styrene-N-isopropylacrylamide) nanospheres, polypyrrole nanospheres, polypyridine polystyrene@poly N-isopropylacrylamide nanospheres, poly(methacrylate-chitosan) nanospheres, poly(methacrylate-N-isopropylacrylamide) nanospheres, and polymethacrylate@poly N-isopropylacrylamide nanospheres; The nanosphere dispersion containing anionic groups on the surface is selected from any one of poly(sodium p-styrene sulfonate) nanospheres, polystyrene@polyacrylic acid nanospheres, polystyrene@poly(methacrylate-acrylic acid) nanospheres, poly(styrene-methyl methacrylate-acrylic acid) nanosphere dispersion, poly(styrene-methyl methacrylate-methacrylic acid) nanospheres, and polyacrylic acid-b-polystyrene nanospheres.

8. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 6, characterized in that: The inorganic nano-microsphere dispersion is selected from any one of ferroferric oxide nano-microspheres and copper oxide nano-microspheres; The inorganic metal-coated nano-microsphere dispersion is selected from any one of nano-microspheres coated with gold on the surface and nano-microspheres coated with nickel on the surface.

9. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: The solid content of the nano-microsphere dispersion is 1% to 25%; the diameter of the nano-microsphere is 130 to 340 nm, and the monodispersity index is less than 0.

08.

10. The optoelectronic dual-mode responsive photonic crystal hydrogel suitable for DLP three-dimensional molding according to claim 1, characterized in that: Place the hydrogel material precursor liquid in the liquid storage tank of the DLP printing equipment; adjust the DLP printing parameters: set the layer thickness to 0.05-0.15 mm, the initial exposure time to 40-70 s, the printing exposure time to 4-9 s, the light-off delay time to 5-16 s, the printing rise height to 5-6 mm, and the motor speed to 0.1-2 mm / s; irradiate and cross-link under any one of the UV-LEDs with a main wavelength of 365, 395, and 405 nm to obtain an optoelectronic dual-mode responsive photonic crystal hydrogel material with a customized three-dimensional structure and structural color effect.

Citation Information

Cited By

  • Zwitterionic polymer-based lithium ion battery electrolyte and preparation method thereof

    CN117175000A

  • Preparation method and application of photoelectric dual-output photonic crystal ionic gel

    CN119875040A

  • Ionic Sulfur Polymer Composite Comprising a Network Formed by Covalent Bonding Between an Ionic Crosslinking Linker and Sulfur, and Manufacturing Method thereof