Phase-change material super-soft high-thermal-conductivity composite material gasket and preparation method thereof
By combining high-thermal phase change gaskets and super-soft thermal gaskets in the thermal gaskets, the problems of incomplete filling and insufficient compression resilience of thermal gaskets are solved, and high thermal conductivity and excellent contact effect are achieved, satisfying the actual situation Application requirements.
Patent Information
- Application Number
- CN202411526087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
AI Technical Summary
Existing thermal conductivity gaskets are difficult to fully fill the air gap between the heating device and the heat sink or the metal base, and cannot meet the needs of compression and resilience while ensuring thermal conductivity.
A phase change material ultra-soft and high thermal conductivity composite gasket was designed. Through the combination of high thermal conductivity phase change gasket and ultra-soft thermal conductivity, the raw material selection and heating conditions are optimized, ensuring that the two are closely combined, and the thermal conductivity is improved. Reduce the interface thermal resistance.
It achieves high thermal conductivity, excellent compression and rebound, and at the same time fully contacts electronic devices, reduces interface thermal resistance, and expands the application range.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal conductive materials, and in particular to a phase change material ultra-flexible high thermal conductive composite material gasket and a preparation method thereof. Background Art
[0002] At present, electronic devices are becoming more miniaturized and integrated. During the use of electronic devices, there is a problem that heat cannot be effectively dissipated, which leads to damage to the electronic devices. Therefore, higher requirements are placed on the heat dissipation of electronic devices. In order to ensure the normal operation of the equipment, heat dissipation devices are required. However, direct contact between heating devices and heat dissipation devices will result in a large contact thermal resistance. The use of thermal conductive pads can effectively fill the gaps between the devices, form a heat conduction path, and improve the thermal conductivity efficiency.
[0003] At present, thermally conductive gaskets are usually prepared with polymer as the matrix and ceramic powder as filler, but they cannot fill the air gap between the heating device and the heat sink or metal base well. In order to solve the above problems, the traditional technology uses phase change thermally conductive gaskets to overcome the incomplete filling problem. For example, Chinese patent application CN117777955A discloses an anti-overflow thermally conductive phase change gasket and its preparation method, which mainly prevents the phase change matrix from overflowing or falling off by introducing a semi-crosslinked support skeleton formed by the reaction of acrylic monomer and photoinitiator into the gasket system. However, due to its conductive properties caused by the metal powder filled in it, its use scenario is limited.
[0004] Therefore, ensuring the compressibility and resilience of the thermally conductive gasket while ensuring sufficient contact between it and the electronic device to meet the actual application requirements is a problem that still needs to be solved. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a phase change material ultra-soft and high thermal conductivity composite gasket. By designing a high thermal conductivity phase change gasket in combination with an ultra-soft thermal conductive gasket, the provided composite gasket can fully contact with electronic devices while ensuring high thermal conductivity, excellent compressibility and resilience, thereby meeting actual use requirements.
[0006] On the one hand, the present invention provides a phase change material ultra-soft high thermal conductivity composite material gasket, which at least includes a high thermal conductivity phase change gasket and an ultra-soft thermal conductive gasket; in terms of weight, the raw materials for preparing the high thermal conductivity phase change gasket include at least: 30-130 parts of thermal conductive powder, 0.5-10 parts of silicone, 0.5-5 parts of phase change wax, and 5-20 parts of polyisobutylene.
[0007] As a preferred technical solution, the raw materials for preparing the ultra-soft thermally conductive gasket include at least 150-300 parts of modified ceramic filler, 2-15 parts of vinyl silicone oil, 0.1-5 parts of methylsiloxane, 0.1-1 parts of hydrogenated silicone oil, 0.1-2 parts of inhibitor, and 0.2-2 parts of catalyst, by weight.
[0008] As a preferred technical solution, the thermally conductive powder is selected from one or a mixture of aluminum powder, angular aluminum oxide, spherical aluminum oxide, single crystal aluminum oxide, aluminum nitride, magnesium oxide, and zinc oxide.
[0009] Preferably, the thermally conductive powder is a combination of aluminum powder, spherical aluminum oxide, and single crystal aluminum oxide.
[0010] Preferably, the mass ratio of the aluminum powder, spherical aluminum oxide and single crystal aluminum oxide is (20-70):(7-50):(3-10), preferably (50-70):(10-30):(5-10).
[0011] Preferably, the particle size of the aluminum powder is 0.1-20 μm, preferably including at least one of 1 μm, 2 μm, 5 μm, 10 μm, and 20 μm.
[0012] Preferably, the particle size of the spherical alumina is 1-70 μm, preferably including at least one of 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 40 μm, and 70 μm.
[0013] Preferably, the particle size of the single crystal aluminum oxide is 0.3-5 μm, preferably including at least one of 0.3 μm, 1.5 μm, 3 μm, and 5 μm.
[0014] As a preferred technical solution, the organosilicon is selected from at least one of the modifiers selected from octyltrimethoxysilane, dodecyltrimethoxysilane, n-octyltriethoxysilane, vinyltrimethoxysilane, and hexamethyldisilazane, preferably octyltrimethoxysilane.
[0015] As a preferred technical solution, the phase change temperature of the phase change wax is 40-125°C, preferably at least one of medium-temperature phase change wax (40-70°C), high-temperature phase change wax (70-100°C), and special phase change wax (70-125°C).
[0016] As a preferred technical solution, the number average molecular weight of the polyisobutylene is 200-2400.
[0017] The preparation method of the modified ceramic filler is as follows: using modification equipment, and using organic siloxane to modify the ceramic filler to obtain the modified ceramic filler.
[0018] As a preferred technical solution, the ceramic filler includes at least 5-20 parts of single crystal alumina, 30-70 parts of spherical alumina, 1-5 parts of zinc oxide, and 20-40 parts of aluminum nitride, by weight.
[0019] Preferably, in parts by weight, the ceramic filler includes: single crystal alumina (1.5 μm, 5 parts; 5 μm, 10 parts), spherical alumina (1 μm, 5 parts; 2 μm, 15 parts; 40 μm, 30 parts), zinc oxide (0.5 μm, 3 parts), and aluminum nitride (20 μm, 5 parts; 120 μm, 27 parts).
[0020] Preferably, the particle size of the zinc oxide is 0.5-3 μm, preferably including at least one of 0.5 μm, 1 μm, and 3 μm.
[0021] Preferably, the particle size of the aluminum nitride is 2-150 μm, preferably including at least one of 2 μm, 10 μm, 20 μm, 80 μm, 100 μm, 120 μm, and 150 μm.
[0022] As a preferred technical solution, the organosiloxane is octyltrimethoxysilane and / or hexamethyldisilazane.
[0023] As a preferred technical solution, the preparation method of the modified ceramic filler is: fill the ceramic filler into the modification equipment, then add organic siloxane, the amount of organic siloxane added is 0.2-5% of the mass of the ceramic filler; close the modification equipment to make its cavity airtight, first use 10-200rpm to stir for 0.5-90min, after the stirring is completed, open the modification equipment, manually scrape off the raised powder, close the modification equipment again, use 150-500rpm to stir for 0.5-30min, after the stirring is completed, pour out the modified filler, bake in an oven at 50-170℃ for 0.5-24h, take out and cool after baking to obtain the modified ceramic filler.
[0024] As a preferred technical solution, the vinyl content in the vinyl silicone oil is 0.08-10wt%, preferably 0.1-0.5wt%.
[0025] Preferably, the vinyl content of the vinyl silicone oil is 0.18wt% (Guangdong Chensi New Material Technology Co., Ltd., cx-352m, single-ended vinyl silicone oil).
[0026] As a preferred technical solution, the methylsiloxane is at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane, preferably hexamethylcyclotrisiloxane.
[0027] As a preferred technical solution, the hydrogen-containing silicone oil is at least one of end hydrogen-containing silicone oil, side hydrogen-containing silicone oil or end-side hydrogen-containing silicone oil.
[0028] Preferably, the hydrogen-containing silicone oil is a combination of terminal hydrogen-containing silicone oil (Shanghai Jingri New Material Technology Co., Ltd., brand DH007) and side hydrogen-containing silicone oil (Shanghai Jingri New Material Technology Co., Ltd., brand H020), and the mass ratio of the terminal hydrogen-containing silicone oil to the side hydrogen-containing silicone oil is (3-8):1, preferably 5:1.
[0029] As a preferred technical solution, the inhibitor is acetylene cyclohexanol.
[0030] As a preferred technical solution, the catalyst is a platinum catalyst.
[0031] The present invention optimizes the raw material selection and addition control of the high thermal conductivity phase change gasket, so that it is tightly combined with the ultra-soft thermal conductive gasket, and the thermal conductivity of the composite phase change material ultra-soft high thermal conductive composite gasket is increased, and the interface thermal resistance is reduced, so as to better meet the actual application requirements. Specifically, the present invention controls the heating conditions and stirring time to disperse the phase change wax into the polyisobutylene system, ensures the uniformity of the phase change system, ensures the subsequent film forming effect, and effectively prevents the problem of melting leakage, while reducing the interface thermal resistance between the phase change material and the device components, better filling the air gap between the heating device and the heat sink or metal base, and expanding the scope of application. However, if the temperature is too low, granular impurities will appear in the subsequent ejected film; if the stirring time is too long, the hardness of the ejected film will increase, and both cannot meet the actual application requirements.
[0032] Furthermore, the introduction of aluminum powder, spherical alumina and single crystal alumina into the high thermal conductivity phase change gasket is controlled. In the presence of silicone, aluminum powder, spherical alumina and single crystal alumina of different particle sizes are combined to ensure the uniformity of the high thermal conductivity phase change gasket, thereby ensuring the subsequent composite effect with the ultra-soft thermal conductive gasket.
[0033] Furthermore, the present invention introduces modified ceramic fillers including single crystal alumina, spherical alumina, zinc oxide, and aluminum nitride by optimizing the ultra-soft thermally conductive gasket, so that the ceramic fillers are evenly dispersed in the polymer system, thereby ensuring that the thermal conductivity of the composite gasket is above 8.8 W / mk.
[0034] Another aspect of the present invention provides a method for preparing a phase change material ultra-flexible high thermal conductivity composite material gasket, which comprises at least the following steps: (1) Stirring and mixing thermal conductive powder, silicone, phase change wax, and polyisobutylene to obtain a phase change base material; (2) Pre-mixing vinyl silicone oil, methylsiloxane, hydrogenated silicone oil, inhibitor, and modified ceramic filler, then adding a catalyst and mixing to obtain a rubber compound, extruding the rubber compound onto a base film, and performing calendering and baking to obtain an ultra-soft thermal conductive gasket; (3) The phase change base material is heated, a diluent is added, stirred and diluted, and then sprayed on the upper surface of the ultra-soft thermal conductive gasket. After natural cooling, a high thermal conductive phase change gasket is formed on the upper surface of the ultra-soft thermal conductive gasket, thereby obtaining an ultra-soft and high thermal conductive composite gasket of the phase change material.
[0035] As a preferred technical solution, the method for preparing the phase change material ultra-flexible high thermal conductivity composite material gasket comprises at least the following steps: (1) Spherical alumina, single crystal alumina, silicone, phase change wax, and polyisobutylene are placed in a stirring kettle, heated to 120-140°C, stirred at 5-30 rpm for 0.1-5 min, and after the stirring, aluminum powder is added three times, stirred at 10-50 rpm for 0.5-30 min, the wall is scraped after the stirring, and stirred again at 10-50 rpm for 0.5-10 min, and vacuum is maintained during the stirring process to obtain a phase change base material; (2) Add vinyl silicone oil, methylsiloxane, hydrogenated silicone oil, inhibitor, and modified ceramic filler into a stirring kettle, stir at 10-50 rpm for 5-30 min, maintain 20-30° C. and start vacuum during stirring, add catalyst after stirring, stir at 30-50 rpm for 1-30 min, start vacuum during stirring and pass cooling water at 10-20° C., scrape the wall after stirring, stir again at 5-20 rpm for 10-120 min, start vacuum during stirring, obtain a rubber compound after stirring, extrude the rubber compound onto a fluoroplastic film using an extrusion plate, calender at a uniform speed, control the oven temperature at 100-130° C., bake for 30-100 min, and control the thickness at 0.3-5 mm to obtain an ultra-soft thermal conductive gasket; (3) Place the phase change base material into a spray kettle and heat it to 90-120°C, add a diluent in an amount of 0.5-50% of the mass of the phase change base material, stir at 10-50 rpm for 0.5-10 min, and then spray it evenly on the upper surface of the ultra-soft thermal conductive gasket. Control the spraying thickness to 10-100 μm, and spray it evenly on the upper surface of the ultra-soft thermal conductive gasket. Naturally cool to 20-30°C to obtain a phase change material ultra-soft high thermal conductive composite gasket.
[0036] As a preferred technical solution, the diluent is a silicone diluent, preferably RH-2001-0.65, Runhe.
[0037] The phase change material ultra-soft high thermal conductivity composite material gasket provided by the present invention has a hardness of up to shore00 5-25, a breakdown voltage greater than 5 kV / mm, and an interface thermal resistance as low as 4°C·cm 2 / W.
[0038] Beneficial Effects 1. The present invention provides a phase change material ultra-soft high thermal conductivity composite gasket. By designing a high thermal conductivity phase change gasket in combination with an ultra-soft thermal conductive gasket, the provided composite gasket can fully contact with electronic devices while ensuring high thermal conductivity and excellent compressibility and resilience, thereby meeting actual use requirements.
[0039] 2. The present invention optimizes the raw material selection and addition amount control of the high thermal conductivity phase change gasket, so that it is tightly bonded with the ultra-soft thermal conductive gasket, while increasing the thermal conductivity of the composite phase change material ultra-soft high thermal conductivity composite gasket and reducing the interface thermal resistance, thereby better meeting the actual application needs.
[0040] 3. The present invention disperses the phase change wax into the polyisobutylene system by controlling the heating conditions and stirring time, thereby ensuring the uniformity of the phase change system and the subsequent film-forming effect, effectively preventing the problem of melting leakage, and reducing the interfacial thermal resistance between the phase change material and the device components, better filling the air gap between the heating device and the heat sink or metal base, and expanding the scope of application.
[0041] 4. The present invention controls the introduction of aluminum powder, spherical alumina and single crystal alumina into the high thermal conductivity phase change gasket. In the presence of silicone, the aluminum powder, spherical alumina and single crystal alumina of different particle sizes are combined to ensure the uniformity of the high thermal conductivity phase change gasket, thereby ensuring the subsequent composite effect with the ultra-soft thermal conductive gasket.
[0042] 5. The present invention introduces modified ceramic fillers including single crystal alumina, spherical alumina, zinc oxide and aluminum nitride by optimizing the ultra-soft thermal conductive gasket, so that the ceramic fillers are evenly dispersed in the polymer system, ensuring that the thermal conductivity of the composite gasket is above 8.8 W / mk. DETAILED DESCRIPTION
[0043] Example 1 Embodiment 1 of the present invention provides, on the one hand, a phase change material ultra-soft high thermal conductivity composite material gasket, including a high thermal conductivity phase change gasket and an ultra-soft thermal conductive gasket; by weight, the raw materials for preparing the high thermal conductivity phase change gasket include: 60 parts of aluminum powder (Angang aluminum powder, 40μm), 5 parts of single crystal alumina (0.3μm), 5 parts of spherical alumina (2μm), 10 parts of spherical alumina (10μm), 0.5 parts of organic silicon, 2 parts of phase change wax, and 15 parts of polyisobutylene. By weight, the raw materials for preparing the ultra-soft thermal conductive gasket include: 200 parts of modified ceramic filler, 5 parts of vinyl silicone oil, 1 part of methylsiloxane, 0.5 parts of hydrogenated silicone oil, 0.1 parts of inhibitor, and 0.2 parts of catalyst.
[0044] The organosilicon is octyltrimethoxysilane.
[0045] The phase change wax is a medium temperature phase change wax (40-70°C, Herun Technology).
[0046] The number average molecular weight of the polyisobutylene is 1200, Guochen Chemical.
[0047] The preparation method of the modified ceramic filler is as follows: fill the ceramic filler into the modification equipment, then add organic siloxane, the addition amount of organic siloxane is 1% of the mass of the ceramic filler; close the modification equipment to make its cavity airtight, first use 100rpm to stir for 20min, open the modification equipment after the stirring, manually scrape off the raised powder, close the modification equipment again, use 300rpm to stir for 10min, pour out the modified filler after the stirring, bake in an oven at 150°C for 3h, take out and cool after baking to obtain the modified ceramic filler.
[0048] In parts by weight, the ceramic filler includes: single crystal alumina (1.5 μm, 5 parts; 5 μm, 10 parts), spherical alumina (1 μm, 5 parts; 2 μm, 15 parts; 40 μm, 30 parts), zinc oxide (0.5 μm, 3 parts), and aluminum nitride (20 μm, 5 parts; 120 μm, 27 parts).
[0049] The organosiloxane is octyltrimethoxysilane.
[0050] The vinyl content of the vinyl silicone oil is 0.18wt% (Guangdong Chensi New Material Technology Co., Ltd., cx-352m, single-ended vinyl silicone oil).
[0051] The methylsiloxane is hexamethylcyclotrisiloxane.
[0052] The hydrogen-containing silicone oil is a combination of end hydrogen-containing silicone oil (Shanghai Jingri New Material Technology Co., Ltd., brand DH007) and side hydrogen-containing silicone oil (Shanghai Jingri New Material Technology Co., Ltd., brand H020), and the mass ratio of the end hydrogen-containing silicone oil to the side hydrogen-containing silicone oil is 5:1.
[0053] The inhibitor is acetylene cyclohexanol.
[0054] The catalyst is a platinum catalyst.
[0055] Embodiment 1 of the present invention provides, on the other hand, a method for preparing a phase change material ultra-flexible high thermal conductive composite material gasket, comprising the following steps: (1) Spherical alumina, single crystal alumina, silicone, phase change wax, and polyisobutylene are placed in a stirring kettle, heated to 130°C, and stirred at 25 rpm for 3 min. After stirring, aluminum powder is added three times, and stirred at 15 rpm for 10 min. After stirring, the wall is scraped, and stirred again at 5 rpm for 10 min. A vacuum is maintained during the stirring process to obtain a phase change base material. (2) Add vinyl silicone oil, methylsiloxane, hydrogenated silicone oil, inhibitor, and modified ceramic filler into a stirring kettle, stir at 10 rpm for 10 min, maintain 25°C and turn on vacuum during stirring, add catalyst after stirring, stir at 30 rpm for 5 min, turn on vacuum during stirring and pass cooling water at 17°C, scrape the wall after stirring, stir again at 10 rpm for 120 min, turn on vacuum during stirring, obtain a rubber compound after stirring, extrude the rubber compound onto a fluoroplastic film using an extrusion plate, calender at a uniform speed, control the oven temperature at 120°C, bake for 40 min, and control the thickness at 0.3 mm to obtain an ultra-soft thermal conductive gasket; (3) Place the phase change base material into a spray kettle and heat it to 100°C, add a diluent in an amount of 20% of the mass of the phase change base material, stir at 30 rpm for 5 minutes, and evenly spray it on the upper surface of the ultra-soft thermal conductive gasket. Control the spraying thickness to 50 μm, and evenly spray it on the upper surface of the ultra-soft thermal conductive gasket. Naturally cool to 25°C to form a high thermal conductivity phase change gasket on the upper surface of the ultra-soft thermal conductive gasket, thereby obtaining a phase change material ultra-soft and high thermal conductivity composite gasket.
[0056] The diluent is an organosilicon diluent, model RH-2001-0.65, Runhe.
[0057] Example 2 Example 2 of the present invention provides a phase change material ultra-flexible high thermal conductivity composite material gasket and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that in step (3), the spraying thickness is controlled to be 80 μm.
[0058] Example 3 Example 3 of the present invention provides a phase change material ultra-flexible high thermal conductivity composite material gasket and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that, in parts by weight, the raw materials for preparing the high thermal conductivity phase change gasket include: 70 parts of aluminum powder (Angang aluminum powder, 40μm), 5 parts of single crystal alumina (0.3μm), 5 parts of spherical alumina (2μm), 5 parts of spherical alumina (10μm), 0.5 parts of silicone, 2 parts of phase change wax, and 15 parts of polyisobutylene.
[0059] Example 4 Example 4 of the present invention provides a phase change material ultra-soft and high thermal conductive composite gasket and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that, by weight, the raw materials for preparing the ultra-soft thermal conductive gasket include: 150 parts of modified ceramic filler, 5 parts of vinyl silicone oil, 1 part of methylsiloxane, 0.8 parts of hydrogenated silicone oil, 0.1 parts of inhibitor, and 0.2 parts of catalyst.
[0060] Example 5 Embodiment 5 of the present invention provides a phase change material ultra-soft high thermal conductivity composite material gasket and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that step (1) is: spherical alumina, single crystal alumina, silicone, phase change wax, and polyisobutylene are placed in a stirring kettle, heated to 100°C, stirred at 25rpm for 3 minutes, and after stirring, aluminum powder is added three times, stirred at 15rpm for 5 minutes, scraped the wall after stirring, and stirred again at 5rpm for 5 minutes, maintaining vacuum during stirring to obtain a phase change base material.
[0061] Example 6 Example 6 of the present invention provides a phase change material ultra-soft high thermal conductivity composite material gasket and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the step (1) is: spherical alumina, single crystal alumina, silicone, phase change wax, and polyisobutylene are placed in a stirring kettle, heated to 100°C, stirred at 25rpm for 3 minutes, and after stirring, aluminum powder is added three times, stirred at 15rpm for 30 minutes, scraped the wall after stirring, and stirred again at 5rpm for 30 minutes, maintaining vacuum during stirring to obtain a phase change base material.
[0062] Comparative Example 1 Comparative Example 1 of the present invention provides a phase change material ultra-flexible and high thermal conductivity composite material gasket and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that, by weight, 60 parts of aluminum powder (Angang aluminum powder, 40 μm) used in the preparation raw materials of the high thermal conductivity phase change gasket are replaced with 60 parts of spherical alumina 40 μm.
[0063] Comparative Example 2 Comparative Example 2 of the present invention provides a phase change material ultra-flexible high thermal conductivity composite gasket and a preparation method thereof. Its specific implementation method is the same as that of Example 1, except that, in parts by weight, the raw materials for preparing the high thermal conductivity phase change gasket include: 70 parts of aluminum powder (Angang aluminum powder, 40 μm), 5 parts of single crystal alumina (0.3 μm), 5 parts of aluminum powder (Angang aluminum powder, 2 μm), 5 parts of aluminum powder (Angang aluminum powder, 10 μm), 0.5 parts of silicone, 2 parts of phase change wax, and 15 parts of polyisobutylene.
[0064] Performance Testing The thermal conductivity, hardness, breakdown voltage and interface thermal resistance of the phase change material ultra-flexible high thermal conductivity composite material gasket provided in the embodiment of the present invention are tested as follows. The test results are shown in Table 1.
[0065] (1) Thermal conductivity: measured according to ASTM D 5470-17 using the Ruiling LW-9389 interface material thermal resistance and thermal conductivity measuring device (at 80°C).
[0066] (2) Hardness: Measured according to ASTM D2240 using a shore 00 durometer (at 25°C).
[0067] (3) Interface thermal resistance: Measured according to standard ASTM D 5470-17 using the Ruiling LW-9389 interface material thermal resistance and thermal conductivity measurement device (at 80°C), with a 2mm thick gasket tested at a constant pressure of 10psi.
[0068] (4) Breakdown voltage: measured in accordance with ASTM D 149 using a breakdown voltage tester (at 25°C), using alternating current (AC), a voltage rise rate of 50 V / s, and a leakage current of 10 mA, and the voltage is raised to breakdown for measurement.
[0069] Table 1
[0070] Analysis of the above table shows that the phase change material ultra-flexible high thermal conductivity composite material gasket provided by Examples 1-4 of the present invention simultaneously ensures that the thermal conductivity, hardness, breakdown voltage and interface thermal resistance meet the actual filling application requirements. The preparation process conditions of Examples 5 and 6 are changed relative to those of Examples 1-4, which affects the hardness and interface thermal resistance of the product. The raw materials for the preparation of the high thermal conductivity phase change gaskets of Comparative Examples 1 and 2 are changed relative to those of Examples 1-4, which affects the hardness breakdown voltage and interface thermal resistance of the product.
Claims
1. A phase change material ultra-flexible high thermal conductivity composite material gasket, characterized in that: At least including a high thermal conductivity phase change gasket and an ultra-soft thermal conductive gasket; In parts by weight, the raw materials for preparing the high thermal conductivity phase change gasket include at least: 30-130 parts of thermal conductive powder, 0.5-10 parts of silicone, 0.5-5 parts of phase change wax, and 5-20 parts of polyisobutylene; in parts by weight, the raw materials for preparing the ultra-soft thermal conductive gasket include at least: 150-300 parts of modified ceramic filler, 2-15 parts of vinyl silicone oil, 0.1-5 parts of methylsiloxane, 0.1-1 parts of hydrogen-containing silicone oil, 0.1-2 parts of inhibitor, and 0.2-2 parts of catalyst; the thermal conductive powder is a combination of aluminum powder, spherical alumina, and single crystal alumina.
2. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The particle size of the aluminum powder is 0.1-20 μm, the particle size of the spherical aluminum oxide is 1-70 μm, and the particle size of the single crystal aluminum oxide is 0.3-5 μm.
3. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The hydrogen-containing silicone oil is one or a mixture of terminal hydrogen-containing silicone oil, side hydrogen-containing silicone oil or terminal-side hydrogen-containing silicone oil.
4. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The phase change temperature of the phase change wax is 40-125°C.
5. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The number average molecular weight of the polyisobutylene is 200-2400.
6. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The preparation method of the modified ceramic filler is: using modification equipment to modify the ceramic filler with organic siloxane to obtain the modified ceramic filler, and the ceramic filler comprises at least 5-20 parts of single crystal aluminum oxide, 30-70 parts of spherical aluminum oxide, 1-5 parts of zinc oxide, and 20-40 parts of aluminum nitride by weight.
7. The phase change material ultra-flexible high thermal conductivity composite material gasket according to claim 1, characterized in that: The particle size of the zinc oxide is 0.5-3 μm, and the particle size of the aluminum nitride is 2-150 μm.
8. A method for preparing the phase change material ultra-flexible high thermal conductivity composite material gasket according to any one of claims 1 to 7, characterized in that: At least the following steps are included: (1) Stirring and mixing thermal conductive powder, silicone, phase change wax, and polyisobutylene to obtain a phase change base material; (2) Pre-mixing vinyl silicone oil, methylsiloxane, hydrogenated silicone oil, inhibitor, and modified ceramic filler, then adding a catalyst and mixing to obtain a rubber compound, extruding the rubber compound onto a base film, and performing calendering and baking to obtain an ultra-soft thermal conductive gasket; (3) The phase change base material is heated, a diluent is added, stirred and diluted, and then sprayed on the upper surface of the ultra-soft thermal conductive gasket. After natural cooling, a high thermal conductive phase change gasket is formed on the upper surface of the ultra-soft thermal conductive gasket, thereby obtaining an ultra-soft and high thermal conductive composite gasket of the phase change material.
Citation Information
Patent Citations
Anti-overflow heat-conducting phase change gasket and preparation method thereof
CN117777955A
Energy-storage radiating sheet and production method thereof
CN103545273A
Super-soft high-thermal-conductivity silicone rubber composite material and preparation method thereof
CN112852171A
Low-thermal-resistance phase-change composite heat-conducting insulating sheet and preparation method thereof
CN115972718A
Ultrathin high-thermal-conductivity silica gel film and application thereof
CN118599321A
Cited By
Highly thermally conductive graphene phase change thermal pad and method of making same
CN123025536A