High-temperature-resistant high-gloss varnish coating composition, preparation method thereof and high-temperature-resistant high-gloss varnish coating prepared from high-temperature-resistant high-gloss varnish coating composition
Through two-component coating formula and reasonable coating methods, the performance problems of carbon fiber composite high-gloss varnish coating in high temperature environments are solved, and high transparency, high gloss and weather resistance are achieved. It is suitable for automotive exterior parts and other applications .
Patent Information
- Application Number
- CN202311780704.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The existing carbon fiber composite high-gloss varnish coating is prone to yellowing, wrinkling, cracking, and delamination in high temperature environments. The introduction of functional additives may lead to a decrease in transparency and gloss, making it difficult to meet the needs of vehicles and other vehicles. The high temperature resistance, high transparency and high gloss requirements of the trim.
Using two-component coating formulations, including component A (hydroxy resin, heat stabilizing additive, ultraviolet absorber and light stabilizer) and component B (isocyanate curing agent and solvent), through reasonable proportional mixing and coating methods, Form a high-temperature and high-gloss varnish coating, and use materials such as Irganox 1010 and ultraviolet absorbers such as Tinuvin 400 to improve the weather resistance and light stability of the coating.
It realizes high transparency, high gloss and good high temperature resistance on the surface of carbon fiber composite materials, can maintain the integrity and aesthetics of the coating under high temperature environment, is suitable for automotive exterior parts and other applications, and has low temperature rapid curing and chemical resistance. Product corrosion characteristics.
Smart Images

Figure BDA0004623619490000071 
Figure BDA0004623619490000081 
Figure BDA0004623619490000083
Abstract
Description
Technical Field
[0001] The invention belongs to the field of surface coating of carbon fiber composite materials, and specifically comprises a high-temperature resistant high-gloss varnish coating composition and a preparation method thereof, and a high-temperature resistant high-gloss varnish coating prepared thereby. Background Art
[0002] Carbon fiber composites (CFRP), as a high-strength, high-rigidity lightweight material, are becoming one of the most popular lightweight materials in the fields of automobiles, rail transit vehicles, sports equipment, etc. When carbon fiber composites are used for exterior trims of rail transit, automobiles and other vehicles, they generally need to be painted to achieve the purpose of aesthetics and protection of the substrate. In order to present the special texture weaving effect of carbon fiber, most of the existing technologies use high-gloss varnish transparent coatings to paint carbon fiber composites. With the expansion of the scope of application, the performance requirements of high-gloss varnish transparent coatings in the painting of carbon fiber composites are getting higher and higher.
[0003] For carbon fiber cars, some exterior parts or interior parts are used in a high temperature environment, such as car wheels, engine hoods, exhaust pipes, etc. Therefore, when such automotive carbon fiber parts are used, the varnish coating is required to have high temperature resistance. Currently on the market, the high-gloss varnish coating used in carbon fiber coating is prone to yellowing, wrinkling, cracking, delamination and other problems in the paint film under high temperature environment. In addition, the transparent varnish coating on the surface of the carbon fiber composite material must be able to improve the weather resistance of the substrate, so as to protect the carbon fiber composite material, especially the epoxy-based carbon fiber composite material, from yellowing. Although some functional additives that can improve the thermal performance of coatings have been publicly reported, it is found in actual application that the introduction of these functional additives may bring about adverse effects such as decreased transparency and reduced gloss, and there will be certain compatibility issues when different resin systems are used together with these functional additives.
[0004] In view of this, how to develop a high-temperature resistant high-gloss varnish coating composition that can be used for surface coating of carbon fiber composite materials more efficiently and conveniently, so as to give the carbon fiber composite materials a high-gloss varnish effect while having excellent high-temperature resistance, high transparency, high gloss, chemical corrosion resistance and high weather resistance, thereby eliminating the above-mentioned defects and deficiencies in the prior art and better serving the needs of exterior paint surfaces of vehicles, etc., is a topic that needs to be urgently solved by relevant technical personnel in the industry. Summary of the invention
[0005] In view of the above problems existing in the prior art, the first object of the present invention is to provide a high temperature resistant high gloss varnish coating composition for carbon fiber composite materials.
[0006] The second object of the present invention is to provide a method for preparing the high temperature resistant high gloss varnish coating composition as described above.
[0007] The third object of the present invention is to provide a high-temperature resistant high-gloss varnish coating prepared using the high-temperature resistant high-gloss varnish coating composition as described above.
[0008] To achieve the above first object, the technical solution adopted by the present invention includes:
[0009] The present invention discloses a high-temperature resistant high-gloss varnish coating composition for carbon fiber composite materials, comprising component A and component B;
[0010] In parts by weight, the component A comprises 50-80 parts of a hydroxyl resin, 10-35 parts of a first solvent, 0.1-2 parts of a heat stabilizing agent, 0.5-3 parts of an ultraviolet light absorber, and 0.5-2 parts of a light stabilizer; the component B comprises 40-90 parts of an isocyanate curing agent and 10-60 parts of a second solvent;
[0011] The weight ratio of component A to component B is 1:10-20:1.
[0012] Furthermore, the heat stabilizing agent is selected from polyhydric hindered phenol antioxidants and / or organic phosphate antioxidants.
[0013] Furthermore, the heat stabilizing agent is selected from one or more of Irganox 1010, Irganox 1076, RIANOX 1010, RIANOX 1076, RIANOX 1098, IRGAFOS 168, and RIANOX 168.
[0014] Furthermore, the hydroxy resin is selected from one or more of hydroxyl-containing acrylic resin, hydroxyl-containing polyester resin, and hydroxyl-containing silicone resin; preferably hydroxyl-containing acrylic resin and / or hydroxyl-containing silicone resin.
[0015] The isocyanate curing agent is selected from one or more of aliphatic isocyanate monomers, aliphatic isocyanate polymers, alicyclic isocyanate monomers, alicyclic isocyanate polymers, aromatic isocyanate monomers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers.
[0016] Further, the first solvent and the second solvent are the same or different, and are independently selected from one or more of hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, 3-ethoxypropionic acid ethyl ester, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, and No. 200 solvent oil.
[0017] Furthermore, the component A further comprises 0.1-2 parts of other auxiliary agents;
[0018] The other additives are selected from one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive.
[0019] Furthermore, the viscosity of the high temperature resistant high gloss varnish coating composition at 23° C. is in the range of 100-20000 mPa·s; preferably 100-10000 mPa·s; and more preferably 100-5000 mPa·s.
[0020] To achieve the above second purpose, the technical solution adopted by the present invention includes:
[0021] The present invention discloses a method for preparing the high temperature resistant high gloss varnish coating composition as described above, comprising the following steps:
[0022] (1) adding a hydroxy resin, a heat stabilizing agent, an ultraviolet light absorber, a light stabilizer and a first solvent into a container A under stirring, and mixing them uniformly to obtain the component A;
[0023] (2) adding an isocyanate curing agent and a second solvent into container B under stirring, and mixing them evenly to obtain component B;
[0024] (3) Component A and component B are mixed in proportion to obtain the high temperature resistant high gloss varnish coating composition.
[0025] To achieve the third objective, the technical solution adopted by the present invention includes:
[0026] The invention discloses a high-temperature resistant high-gloss varnish coating. At least one layer of the high-temperature resistant high-gloss varnish coating composition as described above is coated on at least one surface of a carbon fiber composite material to obtain the high-temperature resistant high-gloss varnish coating.
[0027] Furthermore, the coating method is selected from air spraying, airless spraying, online electrostatic spraying or in-mold coating.
[0028] Beneficial effects of the present invention:
[0029] Compared with the prior art, the technical solution provided by the present invention has the following advantages:
[0030] The high-temperature resistant high-gloss varnish coating composition of the present invention can give the carbon fiber composite material high transparency and beautiful high-gloss varnish effect, and enable the carbon fiber composite material to meet the high-temperature resistance performance requirements of automobile exteriors.
[0031] The high temperature resistant high gloss varnish coating composition of the present invention has good weather resistance, and can play a good protective role on the surface of carbon fiber composite materials after adding ultraviolet light absorber and light stabilizer.
[0032] The high temperature resistant high gloss varnish coating composition of the present invention has the characteristics of high gloss, low temperature rapid curing, chemical corrosion resistance, etc., and can meet the application requirements of carbon fiber composite materials such as automobile exterior parts. DETAILED DESCRIPTION
[0033] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the case of illustrating and explaining the purpose of the present invention through the following examples, the components of the composition are explained in parts by weight as a general standard. Unless otherwise specified, for the sake of simplicity, the "parts" described in the examples of the present invention have the same meaning as parts by weight.
[0035] The first aspect of the present invention provides a high-temperature resistant high-gloss varnish coating composition for carbon fiber composite materials, which improves the high-temperature resistance of the formed coating by introducing a heat-stabilizing additive into the two-component coating formula. The specific formula of the high-temperature resistant high-gloss varnish coating composition is:
[0036] Comprising component A and component B;
[0037] In parts by weight, the component A comprises 50-80 parts of a hydroxyl resin, 10-35 parts of a first solvent, 0.1-2 parts of a heat stabilizing agent, 0.5-3 parts of an ultraviolet light absorber, and 0.5-2 parts of a light stabilizer; the component B comprises 40-90 parts of an isocyanate curing agent and 10-60 parts of a second solvent;
[0038] The weight ratio of component A to component B is 1:10-20:1.
[0039] Furthermore, the heat stabilizing agent is selected from a polyhedral hindered phenol antioxidant and / or an organic phosphate antioxidant; although these heat stabilizing agents currently reported can improve the heat resistance of the coating to a certain extent, they may also sacrifice a certain degree of transparency and gloss. Considering the application scenarios of the high temperature resistant high gloss varnish coating composition of the present invention, the requirements for performance such as transparency and gloss are also very high, so it is necessary to screen out a heat stabilizing agent that is suitable for the application requirements of the present invention and is adapted to the coating system of the present invention. After a large number of experimental studies by the inventors, when the heat stabilizing agent is selected from one or more of Irganox 1010, Irganox 1076, RIANOX 1010, RIANOX 1076, RIANOX 1098, IRGAFOS168, and RIANOX168, the prepared varnish coating has better comprehensive performance. Preferably, the amount of the heat stabilizing agent in component A may be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0 parts, etc.
[0040] Furthermore, the hydroxyl resin is selected from one or more of hydroxyl-containing acrylic resins, hydroxyl-containing polyester resins, and hydroxyl-containing silicone resins. Experiments have found that for the coating composition formula provided by the present invention, when the hydroxyl resin is selected from hydroxyl-containing acrylic resins and / or hydroxyl-containing silicone resins, the coating obtained thereby has better comprehensive performance.
[0041] Further, the hydroxyl-containing acrylic resin is polymerized from acrylic acid monomers, methacrylic acid monomers or derivatives thereof. For example, the hydroxyl-containing acrylic resin includes but is not limited to Setalux 1907BA-75, TIRES2850, SETALUX 1774SS-65, SETALUX 1215BA-68, SETALUX 1274BA-70, SETALUX 91757VX-60, SETALUX 91795VX-60, SETALUX 61767VX-60, etc., commercially available from Allnex, or Joncryl 507, Joncryl 804, Joncryl 910, etc., commercially available from BASF.
[0042] Furthermore, the hydroxyl-containing silicone resin includes but is not limited to the commercially available silicone resins from EVONIK. E900, E 901, etc., or commercially available from WACKER MSE 100, or the one sold by Jiazhi JZ-9522, JZ-9540, etc.
[0043] Further, the hydroxyl-containing polyester resin includes but is not limited to conventional saturated polyester polyols, polycaprolactone polyols, polycarbonate diols, etc. For example, it can be SETAL 1612VS-60, SETAL 1715VX-74, SETAL 90173SS-50, SETAL 1603BA-78, SETAL 168SS-80, SETAL 82166SS-64, etc. commercially available from Allnex, or K-Flex XM-332, K-Flex 148, K-Flex XM-337, etc. commercially available from King Industries.
[0044] Further, the component A comprises 60-75 parts of hydroxyl resin; illustratively, it can be 60 parts, 60.5 parts, 61 parts, 61.5 parts, 62 parts, 62.5 parts, 63 parts, 63.5 parts, 64 parts, 64.5 parts, 65 parts, 65.5 parts, 66 parts, 66.5 parts, 67 parts, 67.5 parts, 68 parts, 68.5 parts, 69 parts, 69.5 parts, 70 parts, 70.5 parts, 71 parts, 71.5 parts, 72 parts, 72.5 parts, 73 parts, 73.5 parts, 74 parts, 74.5 parts or 75 parts, and the like.
[0045] Furthermore, the isocyanate curing agent includes, but is not limited to, one or more of aliphatic isocyanate monomers, aliphatic isocyanate polymers, alicyclic isocyanate monomers, alicyclic isocyanate polymers, aromatic isocyanate monomers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers.
[0046] Furthermore, the aliphatic isocyanate monomer includes, but is not limited to, one or more of tetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate, 2,2,4-trimethylhexane 1,6-diisocyanate, ethylene diisocyanate, and 1,12-dodecane diisocyanate.
[0047] Furthermore, the aliphatic isocyanate polymer is an aliphatic isocyanate dimer and / or an aliphatic isocyanate trimer.
[0048] Furthermore, the alicyclic isocyanate monomer includes but is not limited to one or more of isophorone diisocyanate, cyclobutane 1,3-diisocyanate, cyclohexane 1,3-diisocyanate, cyclohexane 1,4-diisocyanate, methylcyclohexyl diisocyanate, 4,4'-methylene dicyclohexyl diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0049] Furthermore, the alicyclic isocyanate polymer is an alicyclic isocyanate dimer and / or an alicyclic isocyanate trimer.
[0050] Furthermore, the aromatic isocyanate monomer includes but is not limited to one or more of toluene 2,4-diisocyanate, toluene 2,6-diisocyanate, diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate, p-phenylene diisocyanate, biphenyl diisocyanate, 3,3'-dimethyl-4,4'-diphenylene diisocyanate, and hexahydrophenylene 1,3-diisocyanate.
[0051] Furthermore, the aromatic isocyanate polymer is an aromatic isocyanate dimer and / or an aromatic isocyanate trimer.
[0052] Furthermore, the isocyanate hybrid polymer is an isocyanate hybrid dimer and / or an isocyanate hybrid trimer.
[0053] Further, the isocyanate curing agent can be any commercially available isocyanate curing agent that meets the above description, including but not limited to Desmodur N 3300, Desmodur N 3390, Desmodur N3600, Desmodur N 3900, Desmodur Z 4470, etc. commercially available from Bayer MaterialScience, or HDT-90, HDT-100, HDT-LV, etc. commercially available from Rhodia Group, or Basonat HI100, etc. commercially available from BASF.
[0054] Further, component A contains 50-80 parts of isocyanate curing agent; illustratively, it can be 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts or 80 parts, etc.
[0055] Further, the ultraviolet light absorber includes but is not limited to one or more of Tinuvin 328, Tinuvin 384-2, Tinuvin 900, Tinuvin 928, Tinuvin 1130, Tinuvin 400, Tinuvin 479, Tinuvin 477, and Tinuvin CarboProtect. Preferably, the component A contains 0.5-1.5 parts of ultraviolet light absorber; illustratively, it can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, or 1.5 parts, etc.
[0056] Further, the light stabilizer includes but is not limited to one or more of Tinuvin 144, Tinuvin 123, Tinuvin 292, Tinuvin 440 and Tinuvin 622. Preferably, the component A contains 0.5-1.0 parts of light stabilizer; illustratively, it can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts or 1.0 parts, etc.
[0057] Furthermore, the component A further comprises 0.1-2 parts of other additives, including but not limited to one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive. It should be understood by those skilled in the art that the additives can be selected according to actual process requirements, and the scope of other additives that can be used in the present invention is not limited to the additives listed above.
[0058] Furthermore, component A may contain 0.01-0.1 parts of a drying agent; component A may contain 0.01-0.3 parts of a substrate wetting agent; component A may contain 0.01-0.2 parts of a wetting and dispersing agent; component A may contain 0.01-0.5 parts of a leveling agent; and component A may contain 0.1-1.0 parts of a rheological additive.
[0059] Further, the first solvent and the second solvent may be the same or different, including but not limited to hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, 3-ethoxypropionic acid ethyl ester, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, No. 200 solvent oil, etc.
[0060] Further, the weight ratio of component A to component B is 1-2:1-2; illustratively, the weight ratio of component A to component B can be 1:1, 5:4, 5:3, 2:1, 4:5, 3:5, 1:2, etc.
[0061] The second aspect of the present invention provides a method for preparing the high temperature resistant high gloss varnish coating composition according to the first aspect of the present invention, comprising the steps of:
[0062] (1) Preparation of component A
[0063] Under stirring, add 50-80 parts of hydroxyl resin, 0.1-2 parts of heat stabilizing agent, 0.5-3 parts of ultraviolet light absorber, 0.5-2 parts of light stabilizer, 0.1-2 parts of other additives and 10-35 parts of the first solvent into container A, mix well, and obtain component A;
[0064] (2) Preparation of component B
[0065] Under stirring, 40-90 parts of an isocyanate curing agent and 10-60 parts of a second solvent are added to container B, wherein the second solvent is pre-filled with an inert gas to eliminate the influence of oxygen, and after mixing evenly, component B is obtained;
[0066] (3) Component A and component B are fully mixed in a weight ratio of 1:10-20:1 to obtain the high temperature resistant high gloss varnish coating composition.
[0067] Furthermore, the viscosity of the high temperature resistant high gloss varnish coating composition at 23° C. is in the range of 100-20000 mPa·s; preferably 100-10000 mPa·s; and more preferably 100-5000 mPa·s.
[0068] The third aspect of the present invention provides a high-temperature resistant high-gloss varnish coating prepared using the high-temperature resistant high-gloss varnish coating composition described in the first aspect of the present invention. The high-temperature resistant high-gloss varnish coating composition is applied to at least one surface of a carbon fiber composite material, especially an epoxy-based carbon fiber composite material substrate, and cured at 60-90°C for 40-80 minutes. The above coating and curing operations are repeated 1-4 times to obtain a high-temperature resistant high-gloss varnish coating.
[0069] Furthermore, the coating thickness formed by the single coating is 40-60 μm; the dry film thickness of the high temperature resistant high gloss varnish coating is 100-200 μm.
[0070] The specific embodiments of the present invention are described in detail below.
[0071] Example 1
[0072] In this embodiment, a high temperature resistant high gloss varnish coating composition is provided, and the high temperature resistant high gloss varnish coating composition includes component A and component B. The compositions of component A and component B in parts by weight are shown in Table 1.1 and Table 1.2.
[0073] Table 1.1 Composition of component A in Example 1
[0074] Components name Number of copies Hydroxyl resin SETALUX 1774 SS-65 69.5 Heat Stabilizer Irganox 1076 0.5 First solvent 1 Butyl acetate 18 First solvent 2 Xylene 10 Substrate wetting agent Tego Wet 270 0.3 Leveling agent BYK-315N 0.2 UV absorber Tinuvin 400 1 Light Stabilizer Tinuvin 123 0.5
[0075] Table 1.2 Composition of component B in Example 1
[0076] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0077] The specific steps of the preparation method and application of the above-mentioned high temperature resistant high gloss varnish coating composition are as follows:
[0078] (1) Under stirring, add SETALUX 1774SS-65, Irganox 1076, butyl acetate and xylene into the main container in sequence, stir for 15-20 minutes, and control the stirring rate at 500-1500 rpm to mix them evenly. Then, add TegoWet 270, BYK-315N, Tinuvin 400 and Tinuvin 123, and continue stirring for 20-30 minutes to obtain component A.
[0079] (2) Under stirring, butyl acetate and propylene glycol methyl ether acetate are added to another container, and nitrogen is introduced. Desmodur N 3390 is added and stirred for 10-20 minutes at a stirring rate of 300-1000 rpm to obtain component B.
[0080] (3) When in use, component A and component B are fully mixed at a weight ratio of 2:1 to obtain the high temperature resistant high gloss varnish coating composition with a viscosity of 100 mPa.s / 23°C.
[0081] (4) The high-temperature resistant high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0082] Example 2
[0083] In this embodiment, a high temperature resistant high gloss varnish coating composition is provided, and the high temperature resistant high gloss varnish coating composition includes component A and component B. The compositions of component A and component B in parts by weight are shown in Table 2.1 and Table 2.2.
[0084] Table 2.1 Composition of component A in Example 2
[0085] Components name Number of copies Hydroxyl resin SETAL 168 SS-80 69.5 Heat Stabilizer Irganox 1076 0.5 First solvent 1 Butyl acetate 18 First solvent 2 Xylene 10 Substrate wetting agent Tego Wet 270 0.3 Leveling agent BYK-315N 0.2 UV absorber Tinuvin 400 1 Light Stabilizer Tinuvin 123 0.5
[0086] Table 2.2 Composition of component B in Example 2
[0087] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0088] The specific steps of the preparation method and application of the above-mentioned high temperature resistant high gloss varnish coating composition are as follows:
[0089] (1) Under stirring, add SETAL 168SS-80, Irganox 1076, butyl acetate and xylene into the main container in sequence, stir for 15-20 minutes, and control the stirring rate at 500-1500 rpm to mix them evenly. Then, add Tego Wet270, BYK-315N, Tinuvin 400 and Tinuvin 123, and continue stirring for 20-30 minutes to obtain component A.
[0090] (2) Under stirring, butyl acetate and propylene glycol methyl ether acetate are added to another container, and nitrogen is introduced. The isocyanate curing agent Desmodur N 3390 is added and stirred for 10-20 minutes at a stirring rate of 300-1000 rpm to obtain component B.
[0091] (3) When in use, component A and component B are fully mixed at a weight ratio of 5:3 to obtain the high temperature resistant high gloss varnish coating composition having a viscosity of 150 mPa.s / 23°C.
[0092] (4) The high-temperature resistant high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0093] Example 3
[0094] In this embodiment, a high temperature resistant high gloss varnish coating composition is provided, and the high temperature resistant high gloss varnish coating composition includes component A and component B. The compositions of component A and component B in parts by weight are shown in Table 3.1 and Table 3.2.
[0095] Table 3.1 Composition of component A in Example 3
[0096]
[0097]
[0098] Table 3.2 Composition of component B in Example 3
[0099] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0100] The specific steps of the preparation method and application of the above-mentioned high temperature resistant high gloss varnish coating composition are as follows:
[0101] (1) Add the following into the main container in sequence while stirring: E 901, Irganox 1076, butyl acetate and xylene are stirred for 15-20 minutes at a stirring rate of 500-1500 rpm to mix them evenly, and then TegoWet 270, BYK-315N, Tinuvin 400 and Tinuvin 123 are added and stirred for 20-30 minutes to obtain component A.
[0102] (2) Under stirring, butyl acetate and propylene glycol methyl ether acetate are added to another container, and nitrogen is introduced. Desmodur N 3390 is added and stirred for 10-20 minutes at a stirring rate of 300-1000 rpm to obtain component B.
[0103] (3) When in use, component A and component B are fully mixed at a weight ratio of 5:4 to obtain the high temperature resistant high gloss varnish coating composition having a viscosity of 150 mPa.s / 23°C.
[0104] (4) The high-temperature resistant high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0105] Example 4
[0106] In this embodiment, a high temperature resistant high gloss varnish coating composition is provided, and the high temperature resistant high gloss varnish coating composition includes component A and component B. The compositions of component A and component B in parts by weight are shown in Table 4.1 and Table 4.2.
[0107] Table 4.1 Composition of component A in Example 4
[0108]
[0109] Table 4.2 Composition of component B in Example 4
[0110] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0111] The specific steps of the preparation method and application of the above-mentioned high temperature resistant high gloss varnish coating composition are as follows:
[0112] (1) Under stirring, add SETALUX 1774SS-65, RIANOX168, butyl acetate and xylene into the main container in sequence, stir for 15-20 minutes, and control the stirring rate at 500-1500 rpm to mix them evenly. Then, add Tego Wet270, BYK-315N, Tinuvin 400 and Tinuvin 123, and continue stirring for 20-30 minutes to obtain component A.
[0113] (2) Under stirring, butyl acetate and propylene glycol methyl ether acetate are added to another container, and nitrogen is introduced. The isocyanate curing agent Desmodur N 3390 is added and stirred for 10-20 minutes at a stirring rate of 300-1000 rpm to obtain component B.
[0114] (3) When in use, component A and component B are fully mixed at a weight ratio of 2:1 to obtain the high temperature resistant high gloss varnish coating composition having a viscosity of 100 mPa.s / 23°C.
[0115] (4) The high-temperature resistant high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0116] Comparative Example 1
[0117] In this comparative example, a high-gloss varnish coating composition is provided, and the high-gloss varnish coating composition comprises component A and component B. The compositions of component A and component B in parts by weight are shown in Table 5.1 and Table 5.2.
[0118] Table 5.1 Composition of component A in comparative example 1
[0119] Components name Number of copies Hydroxyl resin SETALUX 1774 SS-65 65 Heat Stabilizer Irganox 1076 5 First solvent 1 Butyl acetate 18 First solvent 2 Xylene 10 Substrate wetting agent Tego Wet 270 0.3 Leveling agent BYK-315N 0.2 UV absorber Tinuvin 400 1 Light Stabilizer Tinuvin 123 0.5
[0120] Table 5.2 Composition of component B in comparative example 1
[0121] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0122] The specific steps of the preparation method and application of the above-mentioned high-gloss varnish coating composition are as follows:
[0123] (1) Under stirring, add SETALUX 1774SS-65, Irganox 1076, butyl acetate and xylene into the main container in sequence, stir for 15-20 minutes, and control the stirring rate at 500-1500 rpm to mix them evenly. Then, add TegoWet 270, BYK-315N, Tinuvin 400 and Tinuvin 123, and continue stirring for 20-30 minutes to obtain component A.
[0124] (2) Under stirring, butyl acetate and propylene glycol methyl ether acetate are added to another container, and nitrogen is introduced. The isocyanate curing agent Desmodur N 3390 is added and stirred for 10-20 minutes at a stirring rate of 300-1000 rpm to obtain component B.
[0125] (3) When in use, component A and component B are fully mixed at a weight ratio of 2:1 to obtain the high gloss varnish coating composition having a viscosity of 120 mPa.s / 23°C.
[0126] (4) The high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0127] Comparative Example 2
[0128] In this comparative example, a high-gloss varnish coating composition is provided, which comprises component A and component B. The compositions of component A and component B in parts by weight are shown in Table 6.1 and Table 6.2.
[0129] Table 6.1 Composition of component A in comparative example 2
[0130] Components name Number of copies Hydroxyl resin SETALUX 1774 SS-65 69.5 Heat Stabilizer Tribasic lead sulfate 0.5 First solvent 1 Butyl acetate 18 First solvent 2 Xylene 10 Substrate wetting agent Tego Wet 270 0.3 Leveling agent BYK-315N 0.2 UV absorber Tinuvin 400 1 Light Stabilizer Tinuvin 123 0.5
[0131] Table 6.2 Composition of component B in comparative example 2
[0132] Components name Number of copies Isocyanate curing agent Desmodur N 3390 70 Second solvent 1 Butyl acetate 15 Second solvent 2 Propylene glycol methyl ether acetate 15
[0133] The specific steps of the preparation method and application of the above-mentioned high-gloss varnish coating composition are as follows:
[0134] (1) While stirring, add SETALUX 1774SS-65, tribasic lead sulfate, butyl acetate and xylene to the main container in sequence, and stir for 15-20 minutes at a stirring rate of 500-1500 rpm. After the mixture is evenly mixed, add TegoWet 270, BYK-315N, Tinuvin 400 and Tinuvin 123, and continue stirring for 20-30 minutes to obtain component A.
[0135] Under stirring, add butyl acetate and propylene glycol methyl ether acetate into another container, fill with nitrogen, add isocyanate curing agent Desmodur N 3390, stir for 10-20 minutes, and control the stirring rate at 300-1000 rpm to obtain component B.
[0136] (3) When in use, component A and component B are fully mixed at a weight ratio of 2:1 to obtain the high gloss varnish coating composition having a viscosity of 150 mPa.s / 23°C.
[0137] (4) The high-gloss varnish coating composition was coated on the epoxy-based carbon fiber composite material substrate and cured at 80°C for 60 min. The above coating and curing operations were repeated twice to obtain a high-temperature resistant high-gloss varnish coating with a dry film thickness of 150 μm. The relevant results are shown in Table 7.
[0138] Table 7 Performance test results of each coating composition on carbon fiber composite material samples
[0139]
[0140] Comparing the performance of Examples 1-4, in terms of pencil hardness and resistance to 92# gasoline, among the hydroxyl resins, the hydroxyl-containing polyester resin has poorer performance than the hydroxyl-containing acrylic resin and the hydroxyl-containing silicone resin, and cannot meet the requirements. Comparison of Example 1 with Examples 1 and 4 shows that the heat stabilizing agent exceeding a certain range will have an adverse effect on the hardness and adhesion of the paint film. Comparison of Example 2 with Examples 1-4 shows that the heat stabilizing agent (tribasic lead sulfate) commonly used in the market is not suitable for the high-gloss varnish system of the present invention, and will affect the gloss, transparency, appearance, gasoline resistance, etc. of the paint film. Secondly, in terms of long-term high temperature resistance (90°C / 1000 hours) and short-term high temperature resistance (150°C / 2 hours), Example 3 and Example 4 are the best, followed by Example 1, then Example 2 and Comparative Example 1, and the worst is Comparative Example 2, which shows that: first, the addition of heat stabilizing agents helps to improve high temperature resistance; second, in terms of high temperature resistance, hydroxyl-containing silicone resin>hydroxyl-containing acrylic resin>hydroxyl-containing polyester resin, and the addition of hydroxyl-containing polyester resin makes it more difficult for the coating to meet the high temperature resistance requirements; third, the heat stabilizing agents commonly used in the market are not suitable for the high gloss varnish system of the invention, and therefore fail to meet the high temperature resistance performance; fourth, in terms of resistance to 92# gasoline, hydroxyl-containing silicone resin and hydroxyl-containing acrylic resin both meet the requirements, but the hydroxyl-containing polyester resin has poor resistance to 92# gasoline, and the coating exhibits surface wrinkling.
[0141] Again, in terms of the light aging performance of Examples 1-4 and Comparative Examples 1-2, it was found that the hydroxyl-containing polyester resin had worse performance than the hydroxyl-containing silicone resin and the hydroxyl-containing acrylic resin. At the same time, too much heat stabilizing agent would affect the light aging performance of the paint film, and the heat stabilizing agents commonly used in the market were not conducive to the light aging performance of the high gloss varnish system of the present invention.
[0142] The present invention is described in this specification only in more preferred specific embodiments, the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the present invention. Any technical solutions that can be obtained by those skilled in the art through logical analysis, reasoning or limited experiments according to the concept of the present invention should be within the protection scope of the present invention.
Claims
1. A high temperature resistant high gloss varnish coating composition for carbon fiber composite materials, It is characterized in that Comprising component A and component B; In parts by weight, the component A comprises 50-80 parts of a hydroxyl resin, 10-35 parts of a first solvent, 0.1-2 parts of a heat stabilizing agent, 0.5-3 parts of an ultraviolet light absorber, and 0.5-2 parts of a light stabilizer; the component B comprises 40-90 parts of an isocyanate curing agent and 10-60 parts of a second solvent; The weight ratio of component A to component B is 1:10-20:
1.
2. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The heat stabilizing agent is selected from polyhydric hindered phenol antioxidants and / or organic phosphate antioxidants.
3. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The heat stabilizing agent is selected from one or more of Irganox 1010, Irganox 1076, RIANOX 1010, RIANOX 1076, RIANOX 1098, IRGAFOS168, and RIANOX168.
4. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The hydroxy resin is selected from one or more of a hydroxyl-containing acrylic resin, a hydroxyl-containing polyester resin, and a hydroxyl-containing silicone resin; The isocyanate curing agent is selected from one or more of aliphatic isocyanate monomers, aliphatic isocyanate polymers, alicyclic isocyanate monomers, alicyclic isocyanate polymers, aromatic isocyanate monomers, aromatic isocyanate polymers, isocyanate hybrids, and isocyanate hybrid polymers; Preferably, the hydroxyl resin is selected from hydroxyl-containing acrylic resin and / or hydroxyl-containing silicone resin.
5. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The first solvent and the second solvent are the same or different, and are independently selected from one or more of hexane, heptane, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, butyl acetate, ethyl acetate, 3-ethoxypropionic acid ethyl ester, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene carbonate, dimethyl carbonate, No. 100 solvent oil, No. 150 solvent oil, and No. 200 solvent oil.
6. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The component A also contains 0.1-2 parts of other additives; The other additives are selected from one or more of a drying agent, a substrate wetting agent, a wetting and dispersing agent, a leveling agent, and a rheological additive.
7. The high temperature resistant high gloss varnish coating composition according to claim 1, It is characterized in that The viscosity of the high temperature resistant high gloss varnish coating composition at 23° C. is in the range of 100-20000 mPa·s, preferably 100-10000 mPa·s, and more preferably 100-5000 mPa·s.
8. A method for preparing the high temperature resistant high gloss varnish coating composition according to any one of claims 1 to 7, It is characterized in that The following steps are included: (1) adding a hydroxy resin, a heat stabilizing agent, an ultraviolet light absorber, a light stabilizer and a first solvent into a container A under stirring, and mixing them uniformly to obtain the component A; (2) adding an isocyanate curing agent and a second solvent into container B under stirring, and mixing them evenly to obtain component B; (3) Component A and component B are mixed in proportion to obtain the high temperature resistant high gloss varnish coating composition.
9. A high-temperature resistant high-gloss varnish coating, It is characterized in that At least one layer of the high temperature resistant high gloss varnish coating composition according to any one of claims 1 to 7 is coated on at least one surface of the carbon fiber composite material to obtain a high temperature resistant high gloss varnish coating.
10. The high temperature resistant high gloss varnish coating according to claim 9, It is characterized in that The coating method is selected from air spraying, airless spraying, online electrostatic spraying or in-mold coating.
Citation Information
Patent Citations
Curable clear coat component and
CN104449303A
Fast-drying varnish and preparation method thereof
CN108977017A
Ceramic two-component water-resistant anti-bubbling white gloss finish paint and preparation method thereof
CN116463039A
Polyurethane polyurea two-component coating composition as well as preparation method and application thereof
CN116925629A
Cited By
Highlight varnish with ultraviolet aging resistance and wear resistance as well as preparation method and application of highlight varnish
CN119735981A
A high-gloss varnish with UV aging resistance and abrasion resistance, its preparation method, and its application.
CN119735981B