Synthesis method of solvent-free polyurethane adhesive
By introducing modified antibacterial microcapsules and thermally conductive fillers, the hydrolysis and aging problems of polyurethane adhesives under high humidity and high temperature conditions were solved, improving their antibacterial, thermal conductivity and antioxidant properties, and ensuring the stability and performance of the adhesives.
Patent Information
- Application Number
- CN202411246906.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyurethane adhesives are prone to hydrolysis, aging and degradation under high humidity and high temperature conditions, and have insufficient antibacterial and thermal conductivity. In addition, the dispersibility of inorganic nanoparticles such as nano-alumina is poor, which affects the adhesive performance.
A modification method using antibacterial microcapsules and thermally conductive fillers was adopted. The antibacterial microcapsules used cyclodextrin with POSS structure, urea group and carbamate group as wall material, and the thermally conductive filler improved dispersibility and thermal stability by introducing hindered phenol and polymerized carbodiimide structure.
This improved the antibacterial properties, high-temperature resistance, thermal conductivity, and antioxidant properties of polyurethane adhesives, thereby enhancing their stability and performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of adhesives, and in particular to a method for synthesizing a solvent-free polyurethane adhesive. Background Art
[0002] The carbamate and isocyanate groups in polyurethane adhesives have strong polarity and chemical activity, so they have excellent chemical adhesion to smooth surfaces of materials containing active hydrogen such as paper, plastic and metal. Waterborne polyurethane adhesives are also called solvent-free polyurethane adhesives. Compared with solvent-based polyurethane adhesives, they do not emit flammable, explosive and toxic organic solvents, and are safer and more environmentally friendly. Two-component waterborne polyurethane adhesives are one type of solvent-free polyurethane adhesives. They are mainly composed of a waterborne polyol component (component A) containing hydroxyl (OH) and a polyisocyanate component (component B) containing isocyanate groups (NCO) with other special-purpose additives. Components A and B are packaged separately. Mix the two components evenly before use. By adjusting the ratio of components A and B, the strength, curing time and other properties of the polyurethane material can be changed. Additives include desiccants, flame retardants, coupling agents, antioxidants, UV inhibitors, colorants, adhesion promoters, fillers, plasticizers, etc.
[0003] When polyurethane adhesives are used in medical and food processing fields, higher requirements are placed on their antibacterial properties. Previous studies have used cyclodextrin-coated 4-terpene alcohol to form microcapsules to improve the antibacterial properties of polyurethane adhesives. However, the compatibility and dispersibility of the microcapsules with polyurethane adhesives are poor, and 4-terpene alcohol is more volatile under high temperature conditions, which is not conducive to the durability of the antibacterial properties of the adhesive. These problems need to be solved urgently.
[0004] In addition, polyurethane materials are prone to hydrolysis under conditions of high humidity and high temperature, which leads to material aging and reduced strength. They are prone to aging and degradation after being exposed to light, heat, and oxygen, which limits the use of polyurethane adhesives. Monomeric carbodiimides such as 2,6-diisopropylphenylcarbodiimide can be used to improve the hydrolysis resistance of polyurethane materials, but the hydrolysis resistance is still insufficient. Antioxidants such as hindered phenols can improve the anti-oxidation and aging properties of polyurethane materials, but the direct addition of small molecule hindered phenols is prone to migration and cannot effectively resist oxidation and aging. Adhesives used in medical electronic products need not only good bonding properties, but also thermal conductivity to ensure the stability of electronic products. Adding thermal conductive fillers such as nano-alumina helps to improve the thermal conductivity of polyurethane adhesives, but inorganic nanoparticles such as nano-alumina are directly added to polyurethane and have problems such as poor dispersibility and easy agglomeration. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for synthesizing a solvent-free polyurethane adhesive.
[0006] A solvent-free polyurethane adhesive, the preparation of which comprises the following steps: Step S1: Weigh the following raw materials in parts by weight included in component A: 100-110 parts of polyester polyol, 40-50 parts of polyether polyol, 15-25 parts of toluene diisocyanate, and 2-4 parts of molecular sieves; weigh the following raw materials in parts by weight included in component B: 100 parts of 4,4-diphenylmethane diisocyanate, 40-50 parts of polyether polyol, 15-20 parts of antibacterial microcapsules, and 10-12 parts of thermal conductive fillers; Furthermore, in step S1, the molecular weight of the polyester polyol is 2000-3000, and the average functionality is 2-3; the polyether polyol is polyethylene glycol 1000; the molecular sieve is 13X molecular sieve; the molar ratio of the OH functional group of component A to the NCO functional group of component B is 1:1.5-2.0; Step S2: Add the polyester polyol and polyether polyol included in component A to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add toluene diisocyanate under stirring, heat to 80-90° C., stir and react for 4-5 h, then add molecular sieves, stir under vacuum for 30-40 min, and obtain component A; Step S3: adding the polyether polyol included in component B to a reaction kettle, stirring at 110° C. under vacuum for 1 hour, cooling to 50° C., then adding 4,4-diphenylmethane diisocyanate under stirring, heating to 80-90° C. and stirring for reaction for 3-4 hours, then adding antibacterial microcapsules and thermal conductive fillers and stirring under vacuum for 25-35 minutes to obtain component B; Step S4: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1.5-2 hours before use to obtain a solvent-free polyurethane adhesive.
[0007] The preparation of the antibacterial microcapsules comprises the following steps: Step A1: Add 2-methoxy-4-nitrobenzene isocyanate, ethylenediamine cyclodextrin and methanol into a flask, and stir the reaction at room temperature for 3-4 hours to obtain a nitro product; then add the nitro product and ethyl acetate into a three-necked flask, heat to 45-55° C., start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5 hours to obtain an amino product; Further, the dosage ratio of 2-methoxy-4-isocyanatonitrobenzene, ethylenediamine cyclodextrin, and methanol is 25-30 g: 10-12 g: 200-220 mL, and the preparation process of ethylenediamine cyclodextrin refers to the synthesis process of CDen (ethylenediamine cyclodextrin) in Section 2.2.1 of the paper "Synthesis of degradable amphiphilic polyesters containing amino-modified beta-cyclodextrin and its controlled release of proteins and anticancer drugs"; the dosage ratio of nitro product, ethyl acetate, and sodium dithionite is 20-25 g: 70-80 mL: 10-12 g; During the reaction of step A1, the isocyanate group in 2-methoxy-4-nitrobenzene isocyanate reacts rapidly with the amino group in 4-amino-3-methylphenol to generate a nitro product containing a stable urea structure and cyclodextrin; the nitro group in the nitro product is reduced to an amino group to obtain an amino product; Step A2: Add the amino product and γ-glycidyl ether silyl propyl sesquioxane to a round-bottom flask, then add dimethyl sulfoxide, stir and react at 50°C for 24 hours, filter, and dry to obtain a hydroxyl product; mix the hydroxyl product and n-butyl isocyanate, add dilute sulfuric acid solution and methanol, and react at 50°C for 4 hours to obtain a modified cyclodextrin product; Further, the amount ratio of the amino product, γ-glycidyl ether silyl propyl sesquioxane, and dimethyl sulfoxide is 10-12g: 19-23g: 60-70mL; the amount ratio of the hydroxyl product, n-butyl isocyanate, dilute sulfuric acid solution, and methanol is 20-25g: 10-12g: 100mL: 200mL, and the mass fraction of the dilute sulfuric acid solution is 20%; During the reaction of step A2, the amino group of the amino product reacts with the epoxy group of γ-glycidyloxysilylpropylsesquioxane to generate a hydroxyl product; the hydroxyl product reacts with the isocyanate group of n-butyl isocyanate to generate a modified cyclodextrin product containing a POSS structure, a urea structure and a carbamate group; Step A3: adding the modified cyclodextrin product to distilled water and stirring for 30 minutes to obtain solution 1, then adding 4-terpene alcohol to anhydrous ethanol to obtain solution 2, slowly adding solution 2 to solution 1 under stirring, stirring and reacting at 50°C for 3 hours, then placing in a refrigerator at 4°C overnight, extracting with ethyl acetate and freeze-drying for 24 hours to obtain antibacterial microcapsules; Further, the dosage ratio of the modified cyclodextrin product and distilled water is 1 g: 10 mL; the dosage ratio of 4-terpene alcohol and anhydrous ethanol is 1 mL: 1 mL; the dosage ratio of solution 2 and solution 1 is 2.5-3 mL: 12-13 mL; During the reaction of step A3, antibacterial microcapsules were prepared by a saturated aqueous solution method using 4-terpene alcohol as the core material and cyclodextrin containing POSS structure, urea structure and carbamate group as the wall material.
[0008] The preparation of the thermally conductive filler comprises the following steps: Step B1: Add nano-alumina to anhydrous ethanol, ultrasonically disperse for 30 minutes, obtain solution a and add it to a three-necked flask, then add oleic acid to anhydrous ethanol, stir at 50-60°C for 35-45 minutes, obtain solution b and add it to the three-necked flask, start reflux stirring and react at 70-80°C for 1-1.5 hours, then filter, dry and grind to obtain modified alumina; add the modified alumina to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, stir and react at room temperature for 4-5 hours to obtain an epoxy product; Further, the dosage ratio of nano-alumina to anhydrous ethanol is 10 g: 30-40 mL, the dosage ratio of oleic acid to anhydrous ethanol is 0.1 mol: 60-70 mL, the dosage ratio of solution a to solution b is 35-45 mL: 65-75 mL; the dosage ratio of modified alumina, dichloromethane and 3-chloroperoxybenzoic acid is 5-6 g: 90-100 mL: 36-40 g; During the reaction of step B1, oleic acid is used to wet-modify nano-alumina to obtain a modified alumina having an alkane chain with unsaturated double bonds on the surface; the unsaturated double bonds in the modified alumina are oxidized into epoxy groups to obtain an epoxy product; Step B2: In a nitrogen atmosphere, add 3,5-di-tert-butyl-4-hydroxybenzoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10h, then heat to 110-120°C, stir for 1-2h to obtain an alcohol hydroxyl product; Further, the usage ratio of 3,5-di-tert-butyl-4-hydroxybenzoic acid, toluene, pyridine and epoxidation product is 30-35 g: 150-160 mL: 0.10-0.15 mol: 10-12 g; During the reaction of step B2, the carboxyl group of 3,5-di-tert-butyl-4-hydroxybenzoic acid reacts with the epoxy group of the epoxy product to form an alcohol hydroxyl product containing nano-alumina and hindered phenol; Step B3: Add 3,5-dinitrobenzoic acid to DMF, add dichlorothionyl under stirring, reflux and stir at 50°C for 4-5h to obtain an acyl chloride product; add an alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to a flask to obtain a mixed solution c; add the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution d, slowly drop the mixed solution d into the mixed solution c in a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, stir at a constant temperature for 8-10h, then heat to 100-110°C, continue stirring for 1-2h, and distill under reduced pressure to obtain a dinitro product; Further, the dosage ratio of 3,5-dinitrobenzoic acid, DMF, and dichlorothionyl is 0.1 mol: 50-60 mL: 0.12-0.15 mol; the dosage ratio of alcohol hydroxyl product, pyridine, triethylamine, and dimethyl sulfoxide is 5-6 g: 0.01-0.015 mol: 0.1 mol: 20-30 mL; the dosage ratio of acyl chloride product and dimethyl sulfoxide is 25-28 g: 50-60 mL; the dosage ratio of mixed solution c and mixed solution d is 25-35 mL: 55-65 mL; During the reaction of step B3, the carboxyl group of 3,5-dinitrobenzoic acid reacts with thionyl chloride to generate an acyl chloride product; the acyl chloride product then reacts with the hydroxyl group of the alcohol hydroxyl product to generate a dinitro product containing nano-alumina and hindered phenol; Step B4: Add the dinitro product and ethyl acetate into a three-necked flask, heat it to 45-55°C, then add sodium dithionite, and reflux and stir to react for 1-1.5h to obtain a dibasic aromatic primary amine; add xylene into the flask, introduce nitrogen, add a dibasic aromatic primary amine and triphosgene at 75°C, and then heat it to 125°C and continue to react for 3.5h to obtain a dibasic isocyanate; add the dibasic isocyanate into another flask, add a catalyst, introduce nitrogen, heat it to 165°C with stirring, and react at a constant temperature for 12h to obtain a thermal conductive filler; Further, the dosage ratio of the dinitro product, ethyl acetate, and sodium dithionite is 8-10 g: 80-90 mL: 20-25 g; the dosage ratio of xylene, dibasic aromatic primary amine, and triphosgene is 120-130 mL: 22-27 g: 35-40 g; the dosage ratio of dibasic isocyanate and catalyst is 25-30 g: 0.3-0.5 mol, and the catalyst is 3-methyl-1-phenyl-2-phosphopentene-1-oxide; During the reaction of step B4, the nitro group in the dinitro product is reduced to an amino group to obtain a dibasic aromatic primary amine; the amino group of the dibasic aromatic primary amine reacts with triphosgene to generate chloroamide, which is then heated to dehydrochlorinate to generate a dibasic isocyanate; the dibasic isocyanate is catalytically decarbonated to generate a thermally conductive filler containing polymerized carbodiimide.
[0009] Beneficial effects of the invention: The invention discloses a method for synthesizing a solvent-free polyurethane adhesive, wherein the solvent-free polyurethane adhesive is prepared by mixing a hydroxyl (OH)-terminated component A and an isocyanate (NCO)-terminated component B. The component B comprises the following raw materials: 4,4-diphenylmethane diisocyanate, polyether polyol, antibacterial microcapsules, and thermal conductive fillers.
[0010] The synthesized antibacterial microcapsules are prepared by using cyclodextrin containing POSS structure, urea group and carbamate group as wall material, 4-terpene alcohol as core material, and the wall material coating the core material; 4-terpene alcohol is the main active ingredient of tea tree essential oil, and has a good inhibitory effect on bacteria such as Staphylococcus aureus and fungi such as Candida albicans. After being coated with modified cyclodextrin with hydrophobic inner cavity, the antibacterial persistence of highly hydrophobic 4-terpene alcohol is improved; the POSS structure has strong thermal stability and structural stability, so that the antibacterial microcapsules maintain good thermal stability at high temperature, and avoid 4-terpene alcohol from being accelerated volatilized by high heat and losing its antibacterial effect; the urea group and carbamate group have similar molecular chain structures with polyurethane adhesives, so that the compatibility and dispersibility of the antibacterial microcapsules in the adhesive are enhanced, which is more conducive to the performance of the antibacterial microcapsules; therefore, the addition of antibacterial microcapsules makes the polyurethane adhesive have durable antibacterial properties and high temperature resistance.
[0011] The synthesized thermal conductive filler is obtained by introducing hindered phenol and polymerized carbodiimide structures into the surface of nano-alumina through reaction. After the surface of nano-alumina is modified, it is not easy to agglomerate in the matrix and is more evenly dispersed. It can timely disperse the heat generated by electronic products during operation, avoid the adverse effects of accumulated heat on the performance of electronic products and adhesives, and improve the thermal conductivity of adhesives; the hindered phenol structure can terminate the oxidative degradation reaction chain and has a good antioxidant effect, so that the adhesive is not oxidized by light, heat, and oxygen and ages to lose adhesion; polymerized carbodiimide has a higher relative molecular mass and has higher thermal stability and low dosage and high effect advantages compared to monomeric carbodiimide, so that the anti-hydrolysis agent can play a stable role; therefore, adding thermal conductive fillers can improve the thermal conductivity, antioxidant and hydrolysis resistance of solvent-free polyurethane adhesives. DETAILED DESCRIPTION
[0012] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] Embodiment 1: An antibacterial microcapsule, the preparation of which comprises the following steps: Step A1: Add 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol into a flask, stir and react at room temperature for 3 hours to obtain a nitro product; then add the nitro product and ethyl acetate into a three-necked flask, heat to 45°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1 hour to obtain an amino product; the amount ratio of 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol is 25g:10g:200mL, and the amount ratio of nitro product, ethyl acetate and sodium dithionite is 20g:70mL:10g; Step A2: Add the amino product and γ-glycidyloxysilylpropylsesquioxane to a round-bottom flask, then add dimethyl sulfoxide, stir and react at 50°C for 24h, filter and dry to obtain a hydroxyl product; mix the hydroxyl product and n-butyl isocyanate, add dilute sulfuric acid solution and methanol, and react at 50°C for 4h to obtain a modified cyclodextrin product; the amount ratio of the amino product, γ-glycidyloxysilylpropylsesquioxane, and dimethyl sulfoxide is 10g:19g:60mL; the amount ratio of the hydroxyl product, n-butyl isocyanate, dilute sulfuric acid solution, and methanol is 20g:10g:100mL:200mL, and the mass fraction of the dilute sulfuric acid solution is 20%; Step A3: Add the modified cyclodextrin product to distilled water and stir for 30 minutes to obtain solution 1, then add 4-terpene alcohol to anhydrous ethanol to obtain solution 2, slowly add solution 2 to solution 1 under stirring, stir and react at 50°C for 3 hours, then place in a refrigerator at 4°C overnight, extract with ethyl acetate and freeze-dry for 24 hours to obtain antibacterial microcapsules; the dosage ratio of the modified cyclodextrin product and distilled water is 1g:10mL; the dosage ratio of 4-terpene alcohol and anhydrous ethanol is 1mL:1mL; the dosage ratio of solution 2 to solution 1 is 2.5mL:12mL.
[0014] Embodiment 2: An antibacterial microcapsule, the preparation of which comprises the following steps: Step A1: Add 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol into a flask, stir and react at room temperature for 3.5 hours to obtain a nitro product; then add the nitro product and ethyl acetate into a three-necked flask, heat to 50°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1.3 hours to obtain an amino product; the amount ratio of 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol is 28g:11g:210mL, and the amount ratio of nitro product, ethyl acetate and sodium dithionite is 23g:75mL:11g; Step A2: Add the amino product and γ-glycidyloxysilylpropylsesquioxane to a round-bottom flask, then add dimethyl sulfoxide, stir and react at 50°C for 24 hours, filter, and dry to obtain a hydroxyl product; after mixing the hydroxyl product and n-butyl isocyanate, add dilute sulfuric acid solution and methanol, and react at 50°C for 4 hours to obtain a modified cyclodextrin product; the amount ratio of the amino product, γ-glycidyloxysilylpropylsesquioxane, and dimethyl sulfoxide is 11g:21g:65mL; the amount ratio of the hydroxyl product, n-butyl isocyanate, dilute sulfuric acid solution, and methanol is 23g:11g:100mL:200mL, and the mass fraction of the dilute sulfuric acid solution is 20%; Step A3: Add the modified cyclodextrin product to distilled water and stir for 30 minutes to obtain solution 1, then add 4-terpene alcohol to anhydrous ethanol to obtain solution 2, slowly add solution 2 to solution 1 under stirring, stir and react at 50°C for 3 hours, then place in a refrigerator at 4°C overnight, extract with ethyl acetate and freeze-dry for 24 hours to obtain antibacterial microcapsules; the dosage ratio of the modified cyclodextrin product and distilled water is 1g:10mL; the dosage ratio of 4-terpene alcohol and anhydrous ethanol is 1mL:1mL; the dosage ratio of solution 2 to solution 1 is 2.8mL:12mL.
[0015] Embodiment 3: An antibacterial microcapsule, the preparation of which comprises the following steps: Step A1: Add 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol into a flask, stir and react at room temperature for 4 hours to obtain a nitro product; then add the nitro product and ethyl acetate into a three-necked flask, heat to 55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1.5 hours to obtain an amino product; the amount ratio of 2-methoxy-4-nitrobenzeneisocyanate, ethylenediamine cyclodextrin and methanol is 30g:12g:220mL, and the amount ratio of nitro product, ethyl acetate and sodium dithionite is 25g:80mL:12g; Step A2: Add the amino product and γ-glycidyloxysilylpropylsesquioxane to a round-bottom flask, then add dimethyl sulfoxide, stir and react at 50°C for 24 hours, filter and dry to obtain a hydroxyl product; mix the hydroxyl product and n-butyl isocyanate, add dilute sulfuric acid solution and methanol, and react at 50°C for 4 hours to obtain a modified cyclodextrin product; the amount ratio of the amino product, γ-glycidyloxysilylpropylsesquioxane, and dimethyl sulfoxide is 12g:23g:70mL; the amount ratio of the hydroxyl product, n-butyl isocyanate, dilute sulfuric acid solution, and methanol is 25g:12g:100mL:200mL, and the mass fraction of the dilute sulfuric acid solution is 20%; Step A3: Add the modified cyclodextrin product to distilled water and stir for 30 minutes to obtain solution 1, then add 4-terpene alcohol to anhydrous ethanol to obtain solution 2, slowly add solution 2 to solution 1 under stirring, stir and react at 50°C for 3 hours, then place in a refrigerator at 4°C overnight, extract with ethyl acetate and freeze-dry for 24 hours to obtain antibacterial microcapsules; the dosage ratio of the modified cyclodextrin product and distilled water is 1g:10mL; the dosage ratio of 4-terpene alcohol and anhydrous ethanol is 1mL:1mL; the dosage ratio of solution 2 and solution 1 is 3mL:13mL.
[0016] Embodiment 4: A thermally conductive filler, the preparation of which comprises the following steps: Step B1: Add nano-alumina to anhydrous ethanol, ultrasonically disperse for 30 minutes, obtain solution a and add it to a three-necked flask, then add oleic acid to anhydrous ethanol, stir at 50°C for 35 minutes, obtain solution b and add it to the three-necked flask, start reflux stirring and react at 70°C for 1 hour, then filter, dry and grind to obtain modified alumina; add modified alumina to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, stir and react at room temperature for 4 hours to obtain an epoxy product; the dosage ratio of nano-alumina to anhydrous ethanol is 10g:30mL, the dosage ratio of oleic acid to anhydrous ethanol is 0.1mol:60mL, the dosage ratio of solution a to solution b is 35mL:65mL; the dosage ratio of modified alumina, dichloromethane and 3-chloroperoxybenzoic acid is 5g:90mL:36g; Step B2: In a nitrogen atmosphere, add 3,5-di-tert-butyl-4-hydroxybenzoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8h, then heat to 110°C, stir for 1h to obtain an alcohol hydroxyl product; the dosage ratio of 3,5-di-tert-butyl-4-hydroxybenzoic acid, toluene, pyridine and epoxy product is 30g:150mL:0.10mol:10g; Step B3: Add 3,5-dinitrobenzoic acid to DMF, add thionyl chloride under stirring, and reflux and stir at 50°C for 4 hours to obtain an acyl chloride product; add the alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to a flask to obtain a mixed solution c; add the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution d, slowly drop the mixed solution d into the mixed solution c in a 0°C ice water bath, after the dropwise addition is completed, heat to 40°C, stir at constant temperature for 8 hours, and then heat to 100°C. ℃, continue stirring for 1h, and distill under reduced pressure to obtain the dinitro product; the dosage ratio of 3,5-dinitrobenzoic acid, DMF, and dichlorothionyl is 0.1mol:50mL:0.12mol; the dosage ratio of alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 5g:0.01mol:0.1mol:20mL; the dosage ratio of acyl chloride product and dimethyl sulfoxide is 25g:50mL; the dosage ratio of mixed solution c and mixed solution d is 25mL:55mL; Step B4: Add the dinitro product and ethyl acetate into a three-necked flask, heat it to 45°C, then add sodium dithionite, and reflux and stir to react for 1 hour to obtain a dibasic aromatic primary amine; add xylene into the flask, introduce nitrogen, add a dibasic aromatic primary amine and triphosgene at 75°C, then heat it to 125°C and continue to react for 3.5 hours to obtain a dibasic isocyanate; add the dibasic isocyanate into another flask, add a catalyst, introduce nitrogen gas, heated to 165°C with stirring, and reacted at a constant temperature for 12 hours to obtain a thermal conductive filler; the dosage ratio of the dinitro product, ethyl acetate, and sodium dithionite is 8g:80mL:20g; the dosage ratio of xylene, dibasic aromatic primary amine, and triphosgene is 120mL:22g:35g; the dosage ratio of diisocyanate and catalyst is 25g:0.3mol, and the catalyst is 3-methyl-1-phenyl-2-phosphopentene-1-oxide.
[0017] Embodiment 5: A thermally conductive filler, the preparation of which comprises the following steps: Step B1: Add nano-alumina to anhydrous ethanol, ultrasonically disperse for 30 minutes, obtain solution a and add it to a three-necked flask, then add oleic acid to anhydrous ethanol, stir at 55°C for 40 minutes, obtain solution b and add it to the three-necked flask, start reflux stirring and react at 75°C for 1.3 hours, then filter, dry and grind to obtain modified alumina; add modified alumina to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, stir and react at room temperature for 4.5 hours to obtain an epoxy product; the dosage ratio of nano-alumina to anhydrous ethanol is 10g:35mL, the dosage ratio of oleic acid to anhydrous ethanol is 0.1mol:65mL, the dosage ratio of solution a to solution b is 40mL:70mL; the dosage ratio of modified alumina, dichloromethane and 3-chloroperoxybenzoic acid is 5.5g:95mL:38g; Step B2: In a nitrogen atmosphere, add 3,5-di-tert-butyl-4-hydroxybenzoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 9 hours, then heat to 115°C, stir for 1.5 hours to obtain an alcohol hydroxyl product; the amount ratio of 3,5-di-tert-butyl-4-hydroxybenzoic acid, toluene, pyridine and epoxy product is 33g:155mL:0.13mol:11g; Step B3: Add 3,5-dinitrobenzoic acid to DMF, add thionyl chloride under stirring, and reflux and stir at 50°C for 4.5h to obtain an acyl chloride product; add the alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to a flask to obtain a mixed solution c; add the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution d, slowly drop the mixed solution d into the mixed solution c in a 0°C ice water bath, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 9h, and then heat to 105°C. Continue stirring for 1.5h, and distill under reduced pressure to obtain a dinitro product; the dosage ratio of 3,5-dinitrobenzoic acid, DMF, and dichlorothionyl is 0.1mol:55mL:0.13mol; the dosage ratio of alcohol hydroxyl product, pyridine, triethylamine, and dimethyl sulfoxide is 5.5g:0.013mol:0.1mol:25mL; the dosage ratio of acyl chloride product and dimethyl sulfoxide is 26g:55mL; the dosage ratio of mixed solution c and mixed solution d is 30mL:60mL; Step B4: Add the dinitro product and ethyl acetate into a three-necked flask, heat it to 50°C, then add sodium dithionite, and reflux with stirring for 1.3 hours to obtain a dibasic aromatic primary amine; add xylene into the flask, introduce nitrogen, add a dibasic aromatic primary amine and triphosgene at 75°C, then heat it to 125°C and continue to react for 3.5 hours to obtain a dibasic isocyanate; add the dibasic isocyanate into another flask, add a catalyst, and introduce The reaction mixture was stirred under nitrogen and heated to 165°C for 12 hours to obtain a thermally conductive filler. The dosage ratio of the dinitro product, ethyl acetate and sodium dithionite was 9 g:85 mL:23 g. The dosage ratio of xylene, dibasic aromatic primary amine and triphosgene was 125 mL:25 g:38 g. The dosage ratio of the dibasic isocyanate and the catalyst was 28 g:0.4 mol, and the catalyst was 3-methyl-1-phenyl-2-phosphopentene-1-oxide.
[0018] Embodiment 6: A thermally conductive filler, the preparation of which comprises the following steps: Step B1: Add nano-alumina to anhydrous ethanol, ultrasonically disperse for 30 minutes, obtain solution a and add it to a three-necked flask, then add oleic acid to anhydrous ethanol, stir at 60°C for 45 minutes, obtain solution b and add it to the three-necked flask, start reflux stirring and react at 80°C for 1.5 hours, then filter, dry and grind to obtain modified alumina; add modified alumina to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, stir and react at room temperature for 5 hours to obtain an epoxy product; the dosage ratio of nano-alumina to anhydrous ethanol is 10g:40mL, the dosage ratio of oleic acid to anhydrous ethanol is 0.1mol:70mL, the dosage ratio of solution a to solution b is 45mL:75mL; the dosage ratio of modified alumina, dichloromethane and 3-chloroperoxybenzoic acid is 6g:100mL:40g; Step B2: In a nitrogen atmosphere, add 3,5-di-tert-butyl-4-hydroxybenzoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 10 hours, then heat to 120°C, stir for 2 hours to obtain an alcohol hydroxyl product; the dosage ratio of 3,5-di-tert-butyl-4-hydroxybenzoic acid, toluene, pyridine and epoxy product is 35g:160mL:0.15mol:12g; Step B3: Add 3,5-dinitrobenzoic acid to DMF, add dichlorothionyl under stirring, and reflux and stir at 50°C for 5h to obtain an acyl chloride product; add the alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to a flask to obtain a mixed solution c; add the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution d, slowly drop the mixed solution d into the mixed solution c in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, stir at constant temperature for 10h, and then heat to 110 ℃, continue stirring for 2h, and distill under reduced pressure to obtain the dinitro product; the dosage ratio of 3,5-dinitrobenzoic acid, DMF, and dichlorothionyl is 0.1mol:60mL:0.15mol; the dosage ratio of alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 6g:0.015mol:0.1mol:30mL; the dosage ratio of acyl chloride product and dimethyl sulfoxide is 28g:60mL; the dosage ratio of mixed solution c and mixed solution d is 35mL:65mL; Step B4: Add the dinitro product and ethyl acetate into a three-necked flask, heat it to 55°C, then add sodium dithionite, and reflux with stirring for 1.5 hours to obtain a dibasic aromatic primary amine; add xylene into the flask, introduce nitrogen, add a dibasic aromatic primary amine and triphosgene at 75°C, then heat it to 125°C and continue to react for 3.5 hours to obtain a dibasic isocyanate; add the dibasic isocyanate into another flask, add a catalyst, introduce nitrogen gas, heated to 165°C with stirring, and reacted at a constant temperature for 12 hours to obtain a thermal conductive filler; the dosage ratio of the dinitro product, ethyl acetate, and sodium dithionite is 10g:90mL:25g; the dosage ratio of xylene, dibasic aromatic primary amine, and triphosgene is 130mL:27g:40g; the dosage ratio of diisocyanate and catalyst is 30g:0.5mol, and the catalyst is 3-methyl-1-phenyl-2-phosphopentene-1-oxide.
[0019] Embodiment 7: A solvent-free polyurethane adhesive, the preparation of which comprises the following steps: Step S1: Weigh the following raw materials in parts by weight included in component A: 100 parts of polyester polyol, 40 parts of polyether polyol, 15 parts of toluene diisocyanate, and 2 parts of molecular sieve; weigh the following raw materials in parts by weight included in component B: 100 parts of 4,4-diphenylmethane diisocyanate, 40 parts of polyether polyol, 15 parts of antibacterial microcapsules, and 10 parts of thermal conductive fillers; the molecular weight of the polyester polyol in step S1 is 2000, and the average functionality is 2; the polyether polyol is polyethylene glycol 1000; the molecular sieve is 13X molecular sieve; the molar ratio of OH functional groups of component A to NCO functional groups of component B is 1:1.5; Step S2: Add the polyester polyol and polyether polyol included in component A to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add toluene diisocyanate under stirring, heat to 80° C. and stir for 4 h, then add molecular sieves and stir under vacuum for 30 min to obtain component A; Step S3: adding the polyether polyol included in component B to a reaction kettle, stirring at 110° C. under vacuum for 1 h, cooling to 50° C., then adding 4,4-diphenylmethane diisocyanate under stirring, heating to 80° C. and stirring for 3 h, then adding the antibacterial microcapsules obtained in Example 1 and the thermal conductive filler obtained in Example 4 and stirring for 25 min under vacuum to obtain component B; Step S4: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1.5 hours before use to obtain a solvent-free polyurethane adhesive.
[0020] Embodiment 8: A solvent-free polyurethane adhesive, the preparation of which comprises the following steps: Step S1: Weigh the following raw materials in parts by weight included in component A: 105 parts of polyester polyol, 45 parts of polyether polyol, 20 parts of toluene diisocyanate, and 3 parts of molecular sieve; weigh the following raw materials in parts by weight included in component B: 100 parts of 4,4-diphenylmethane diisocyanate, 45 parts of polyether polyol, 18 parts of antibacterial microcapsules, and 11 parts of thermal conductive fillers; the molecular weight of the polyester polyol in step S1 is 2000, and the average functionality is 2; the polyether polyol is polyethylene glycol 1000; the molecular sieve is 13X molecular sieve; the molar ratio of OH functional groups of component A to NCO functional groups of component B is 1:1.8; Step S2: Add the polyester polyol and polyether polyol included in component A to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add toluene diisocyanate under stirring, heat to 85° C. and stir for 4.5 h, then add molecular sieves and stir under vacuum for 35 min to obtain component A; Step S3: Add the polyether polyol included in component B to the reaction kettle, stir at 110° C. under vacuum for 1 hour, cool to 50° C., then add 4,4-diphenylmethane diisocyanate under stirring, heat to 85° C. and stir for 3.5 hours, then add the antibacterial microcapsules obtained in Example 2 and the thermal conductive filler obtained in Example 5 and stir under vacuum for 30 minutes to obtain component B; Step S4: Component A and component B are packaged in double tubes. Before use, components A and B are added to a reaction kettle and stirred for 1.8 hours to obtain a solvent-free polyurethane adhesive.
[0021] Embodiment 9: A solvent-free polyurethane adhesive, the preparation of which comprises the following steps: Step S1: Weigh the following raw materials in parts by weight included in component A: 110 parts of polyester polyol, 50 parts of polyether polyol, 25 parts of toluene diisocyanate, and 4 parts of molecular sieve; weigh the following raw materials in parts by weight included in component B: 100 parts of 4,4-diphenylmethane diisocyanate, 50 parts of polyether polyol, 20 parts of antibacterial microcapsules, and 12 parts of thermal conductive fillers; the molecular weight of the polyester polyol in step S1 is 3000, and the average functionality is 3; the polyether polyol is polyethylene glycol 1000; the molecular sieve is 13X molecular sieve; the molar ratio of OH functional groups of component A to NCO functional groups of component B is 1:2.0; Step S2: Add the polyester polyol and polyether polyol included in component A to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add toluene diisocyanate under stirring, heat to 90° C. and stir for 5 h, then add molecular sieves and stir under vacuum for 40 min to obtain component A; Step S3: adding the polyether polyol included in component B to a reaction kettle, stirring at 110° C. under vacuum for 1 h, cooling to 50° C., then adding 4,4-diphenylmethane diisocyanate under stirring, heating to 90° C. and stirring for 4 h, then adding the antibacterial microcapsules obtained in Example 3 and the thermal conductive filler obtained in Example 6 and stirring for 35 min under vacuum to obtain component B; Step S4: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 2 hours before use to obtain a solvent-free polyurethane adhesive.
[0022] Comparative Example 1: This comparative example is a commercially available solvent-free two-component polyurethane adhesive.
[0023] Comparative Example 2: Compared with Example 9, the modified cyclodextrin product in step A3 is replaced by the nitro product in step A1, that is, the POSS structure and carbamate group are not introduced into the cyclodextrin, and the rest is exactly the same as Example 9 to prepare a solvent-free polyurethane adhesive.
[0024] Comparative Example 3: Compared with Example 9, the thermally conductive filler is replaced with the alcohol hydroxyl product in step B2, that is, the polymerized carbodiimide structure is not introduced, and the rest is exactly the same as Example 9 to prepare a solvent-free polyurethane adhesive.
[0025] The solvent-free polyurethane adhesive prepared by the present invention is further tested for its effect, and the test results are as follows.
[0026] In order to test the solvent-free polyurethane adhesive prepared by the present invention, Escherichia coli, Staphylococcus aureus and Candida albicans are used as experimental bacteria to test the antibacterial property of the solvent-free polyurethane adhesive; the tensile shear strength between the polyurethane adhesive and aluminum and aluminum is tested according to GB / T7124-2008 "Determination of tensile shear strength of adhesives (rigid material to rigid material)", during the test, the aluminum / adhesive / aluminum samples are placed at 25° C. and 90° C. for 72 hours respectively, and then the tensile shear strength is tested; the thermal conductivity of the sample is measured by a thermal conductivity coefficient analyzer based on the hot wire method, and the size of the tested sample is 50mm×50mm×3mm; the obtained solvent-free polyurethane adhesive is placed at a temperature of 25° C. and a strength of 1000W / m 2 After irradiation with ultraviolet light for 72 hours, the tensile shear strength retention rate was tested; the obtained solvent-free polyurethane adhesive was placed at 60°C for hydrolysis for 72 hours, and the tensile shear strength was tested. The results are recorded in Table 1; Table 1: Test results
[0027] According to the data in Table 1, it can be seen from the comparison between Examples 7-9 and Comparative Example 1 that the solvent-free polyurethane adhesive prepared by the present invention has good antibacterial properties, high temperature resistance, thermal conductivity, oxidation resistance and hydrolysis resistance. It can be seen from the comparison between Example 9 and Comparative Example 2 that the introduction of POSS structure into the wall material cyclodextrin of the antibacterial microcapsule is conducive to the improvement of the high temperature resistance of the adhesive, and the introduction of carbamate groups enhances the dispersibility of the antibacterial microcapsules, which is more conducive to the improvement of the antibacterial properties of the adhesive. It can be seen from the comparison between Example 9 and Comparative Example 3 that the use of thermally conductive fillers introduced with polymerized carbodiimide improves the hydrolysis resistance of the adhesive.
[0028] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for synthesizing a solvent-free polyurethane adhesive, characterized in that: The steps include: Step S1: Weigh the following raw materials in parts by weight included in component A: 100-110 parts of polyester polyol, 40-50 parts of polyether polyol, 15-25 parts of toluene diisocyanate, and 2-4 parts of molecular sieves; weigh the following raw materials in parts by weight included in component B: 100 parts of 4,4-diphenylmethane diisocyanate, 40-50 parts of polyether polyol, 15-20 parts of antibacterial microcapsules, and 10-12 parts of thermal conductive fillers; Step S2: Add the polyester polyol and polyether polyol included in component A to a reaction kettle, stir at 110° C. under vacuum for 2 h, cool to 50° C., then add toluene diisocyanate under stirring, heat to 80-90° C., stir and react for 4-5 h, then add molecular sieves, stir under vacuum for 30-40 min, and obtain component A; Step S3: adding the polyether polyol included in component B to a reaction kettle, stirring at 110° C. under vacuum for 1 hour, cooling to 50° C., then adding 4,4-diphenylmethane diisocyanate under stirring, heating to 80-90° C. and stirring for reaction for 3-4 hours, then adding antibacterial microcapsules and thermal conductive fillers and stirring under vacuum for 25-35 minutes to obtain component B; Step S4: Package component A and component B in double tubes, add components A and B into a reaction kettle and stir for 1.5-2 hours before use to obtain a solvent-free polyurethane adhesive.
2. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: The preparation of the antibacterial microcapsules comprises the following steps: Step A1: Add 2-methoxy-4-nitrobenzene isocyanate, ethylenediamine cyclodextrin and methanol into a flask, and stir the reaction at room temperature for 3-4 hours to obtain a nitro product; then add the nitro product and ethyl acetate into a three-necked flask, heat to 45-55° C., start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5 hours to obtain an amino product; Step A2: Add the amino product and γ-glycidyl ether silyl propyl sesquioxane to a round-bottom flask, then add dimethyl sulfoxide, stir and react at 50°C for 24 hours, filter, and dry to obtain a hydroxyl product; mix the hydroxyl product and n-butyl isocyanate, add dilute sulfuric acid solution and methanol, and react at 50°C for 4 hours to obtain a modified cyclodextrin product; Step A3: Add the modified cyclodextrin product to distilled water and stir for 30 minutes to obtain solution 1. Then add 4-terpene alcohol to anhydrous ethanol to obtain solution 2. Slowly add solution 2 to solution 1 under stirring, stir and react at 50°C for 3 hours, then place in a refrigerator at 4°C overnight, extract with ethyl acetate and freeze-dry for 24 hours to obtain antibacterial microcapsules.
3. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: In step A1, the usage ratio of 2-methoxy-4-nitrobenzene isocyanate, ethylenediamine cyclodextrin, and methanol is 25-30 g: 10-12 g: 200-220 mL; the usage ratio of nitro product, ethyl acetate, and sodium dithionite is 20-25 g: 70-80 mL: 10-12 g.
4. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: In step A2, the amount ratio of the amino product, γ-glycidyl ether silyl propyl sesquioxane, and dimethyl sulfoxide is 10-12g:19-23g:60-70mL; the amount ratio of the hydroxyl product, n-butyl isocyanate, dilute sulfuric acid solution and methanol is 20-25g:10-12g:100mL:200mL, and the mass fraction of the dilute sulfuric acid solution is 20%.
5. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: In step A3, the usage ratio of the modified cyclodextrin product and distilled water is 1 g:10 mL; the usage ratio of 4-terpene alcohol and anhydrous ethanol is 1 mL:1 mL; and the usage ratio of solution 2 and solution 1 is 2.5-3 mL:12-13 mL.
6. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: The preparation of the thermally conductive filler comprises the following steps: Step B1: Add nano-alumina to anhydrous ethanol, ultrasonically disperse for 30 minutes, obtain solution a and add it to a three-necked flask, then add oleic acid to anhydrous ethanol, stir at 50-60°C for 35-45 minutes, obtain solution b and add it to the three-necked flask, start reflux stirring and react at 70-80°C for 1-1.5 hours, then filter, dry and grind to obtain modified alumina; Add modified alumina to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, stir and react at room temperature for 4-5 hours to obtain the epoxy product; Step B2: In a nitrogen atmosphere, add 3,5-di-tert-butyl-4-hydroxybenzoic acid and toluene into a flask, heat to 45°C, add pyridine, start stirring, add the epoxy product into the flask, stir and react for 8-10h, then heat to 110-120°C, stir for 1-2h to obtain an alcohol hydroxyl product; Step B3: Add 3,5-dinitrobenzoic acid to DMF, add thionyl chloride under stirring, and reflux and stir at 50° C. for 4-5 hours to obtain an acyl chloride product; Add the alcohol hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution c; add the acyl chloride product into dimethyl sulfoxide to obtain a mixed solution d, slowly drop the mixed solution d into the mixed solution c in a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, stir at constant temperature for 8-10h, then heat to 100-110°C, continue stirring for 1-2h, and distill under reduced pressure to obtain a dinitro product; Step B4: Add the dinitro product and ethyl acetate into a three-necked flask, heat it to 45-55°C, then add sodium dithionite, and reflux with stirring to react for 1-1.5 hours to obtain a dibasic aromatic primary amine; add xylene into the flask, pass nitrogen, add a dibasic aromatic primary amine and triphosgene at 75°C respectively, and then heat it to 125°C and continue to react for 3.5 hours to obtain a dibasic isocyanate; add the dibasic isocyanate into another flask, add a catalyst, pass nitrogen, heat it to 165°C with stirring, and react at a constant temperature for 12 hours to obtain a thermally conductive filler.
7. The method for synthesizing a solvent-free polyurethane adhesive according to claim 6, characterized in that: In step B1, the usage ratio of nano-alumina and anhydrous ethanol is 10g:30-40mL, the usage ratio of oleic acid and anhydrous ethanol is 0.1mol:60-70mL, the usage ratio of solution a and solution b is 35-45mL:65-75mL; the usage ratio of modified alumina, dichloromethane and 3-chloroperbenzoic acid is 5-6g:90-100mL:36-40g; in step B2, the usage ratio of 3,5-di-tert-butyl-4-hydroxybenzoic acid, toluene, pyridine and epoxy product is 30-35g:150-160mL:0.10-0.15mol:10-12g.
8. The method for synthesizing a solvent-free polyurethane adhesive according to claim 6, characterized in that: In step B3, the usage ratio of 3,5-dinitrobenzoic acid, DMF, and dichlorothionyl is 0.1 mol: 50-60 mL: 0.12-0.15 mol; the usage ratio of alcoholic hydroxyl product, pyridine, triethylamine, and dimethyl sulfoxide is 5-6 g: 0.01-0.015mol: 0.1mol: 20-30mL; the usage ratio of the acyl chloride product and dimethyl sulfoxide is 25-28g: 50-60mL; the usage ratio of the mixed solution c and the mixed solution d is 25-35mL: 55-65mL.
9. The method for synthesizing a solvent-free polyurethane adhesive according to claim 6, characterized in that: In step B4, the usage ratio of the dinitro product, ethyl acetate and sodium dithionite is 8-10g:80-90mL:20-25g; the usage ratio of xylene, dibasic aromatic primary amine and triphosgene is 120-130mL:22-27g:35-40g; the usage ratio of dibasic isocyanate and catalyst is 25-30g:0.3-0.5mol, and the catalyst is 3-methyl-1-phenyl-2-phosphopentene-1-oxide.
10. The method for synthesizing a solvent-free polyurethane adhesive according to claim 1, characterized in that: In step S1, the molecular weight of the polyester polyol is 2000-3000, and the average functionality is 2-3; the polyether polyol is polyethylene glycol 1000; the molecular sieve is 13X molecular sieve; and the molar ratio of the OH functional group of component A to the NCO functional group of component B is 1:1.5-2.0.
Citation Information
Patent Citations
Modified PBS foaming material and preparation method thereof
CN118271810A
Temperature-resistant high-viscosity adhesive and preparation method thereof
CN118421255A
Cited By
OCA optical film and preparation method thereof
CN119471867A
Multi-layer composite adhesive tape and preparation method thereof
CN120209725A
Multilayer composite tape and preparation method thereof
CN120209725B