Hydrogen-rich smelting method adopting high-proportion lump ore
Through the hydrogen-rich smelting method of high proportion block ore, combined with the blast furnace gas booster transmission and circulating gas vents, hydrogen addition is optimized, which solves the problems of reduced air permeability of soft fusion belts and high greenhouse gas emissions in the blast furnace, and achieves higher economic benefits and environmentally friendly.
Patent Information
- Application Number
- CN202411235367.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
The increase in the proportion of natural block ore in existing blast furnaces leads to thickening of the soft fusion belt, reducing breathability, and the use of carbonaceous raw materials leads to excessive greenhouse gas emissions. The existing hydrogen-rich blowing technology cannot effectively replace a large number of carbonaceous raw materials.
Using the hydrogen-rich smelting method of high proportion block ore, the design of blast furnace gas booster conveyor pipe and carbon dioxide adsorption chamber, combined with the circulating gas air vent and hydrogen-rich gas injection port, optimize the hydrogen addition amount and spraying method, and enhance indirect reduction and thermodynamics Recycle and reduce the use of carbonaceous raw materials.
The proportion of natural block ore is increased, the use of carbonaceous raw materials is reduced, carbon dioxide emissions is reduced, the gas thermodynamic cycle of the soft melting belt is optimized, the blast furnace direct movement is ensured, and higher economic benefits and environmental friendliness are achieved.
Smart Images

Figure CN119040533A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of blast furnace ironmaking, and in particular to a hydrogen-rich smelting method using high-proportion lump ore. Background Art
[0002] The existing conventional blast furnace mineral charge structure is mainly about 70wt.% of sintered ore, about 20wt.% of pelletized ore and about 10wt.% of natural lump ore. Such a setting can achieve a good ratio with coke to achieve smooth operation of the blast furnace. Since the overall cost of natural lump ore is relatively low, if the proportion of natural lump ore can be increased, better economic benefits will be generated. However, if the proportion of natural lump ore is increased, the soft melting zone of the blast furnace will become thicker and move upward, thereby reducing the permeability of the blast furnace and affecting the smooth operation of the blast furnace. According to general thinking, if this defect is overcome, it is necessary to increase the amount of high-quality coke added, and this setting increases the amount of coke added, which has a certain impact on the cost. How to increase the proportion of lump ore without increasing the addition of high-quality coke too much has become a research focus.
[0003] At the same time, the steel industry is one of the main contributors to greenhouse gases, with up to 3-8% of carbon dioxide emitted by the steel industry, and in the steel industry, carbon dioxide emitted by blast furnaces accounts for a very large proportion. Since the existing long process mainly uses the blast furnace converter process, and the blast furnace process mainly uses carbonaceous raw materials such as coke and coal powder as reducing agents and fuels, the carbon dioxide content in the blast furnace gas produced by the blast furnace accounts for about 10%.
[0004] To reduce greenhouse gas emissions in blast furnace gas, on the one hand, it is necessary to treat the blast furnace gas, and on the other hand, it is also possible to reduce the proportion of carbonaceous raw materials from the source, thereby reducing the production of carbon dioxide from the source. The emergence of hydrogen-rich injection technology can replace part of the carbonaceous raw materials through hydrogen combustion, thereby reducing the production of carbon dioxide. Hydrogen-rich injection has the characteristics of fast reaction rate, clean products, and small environmental load. However, carbonaceous raw materials can only replace part of them due to their skeleton effect and other related effects, that is, the blast furnace has a limit coke ratio. As the amount of hydrogen-rich gas injected into the blast furnace increases, the replacement ratio gradually decreases, and the utilization rate of hydrogen-rich gas also gradually decreases. Therefore, the proportion of hydrogen-rich injection and the injection method have become the main focus of existing research.
[0005] Chinese patent publication CN217103938U discloses a method for producing a hydrogen-rich fuel gas with low CO 2 The hydrogen-rich carbon blast furnace ironmaking device achieves the effect of reducing carbon dioxide production by injecting hydrogen-rich gas by burning blast furnace gas in a blast heating furnace and using the heat to heat hydrogen-rich gas. However, the technical solution does not refine the injection method of hydrogen-rich injection, and the blast furnace gas only utilizes its combustion performance, without further utilizing its reduction performance. Summary of the invention
[0006] The object of the present invention is to provide a hydrogen-rich smelting method using high-proportion lump ore.
[0007] The specific implementation is through the following technical solutions: A method for smelting hydrogen from high-proportion lump ore is carried out using a high-proportion lump ore hydrogen-rich smelting device, wherein the high-proportion lump ore hydrogen-rich smelting device includes a blast furnace, a blast furnace gas booster transmission pipe, a carbon dioxide adsorption chamber, a slag insulation chamber, a high-temperature gas transmission pipe, a high-temperature gas injection pipe, and a hydrogen-rich gas injection pipe.
[0008] A blast furnace gas exhaust pipe is provided on the top of the blast furnace, and the outlet end of the blast furnace gas exhaust pipe is respectively connected with the inlet end of the blast furnace gas booster transmission pipe and the blast furnace gas exhaust pipe; the blast furnace gas exhaust pipe is connected with an external blast furnace gas treatment device, and a carbon dioxide removal component and a gas pressurization component are provided on the blast furnace gas booster transmission pipe.
[0009] The slag channel of the blast furnace is connected to the entrance of the slag insulation chamber through a pipeline. The slag insulation chamber is arranged above the carbon dioxide adsorption chamber. The slag insulation chamber is a square cavity or a cylindrical cavity made of refractory bricks. A slag release port is opened below the slag insulation chamber, and the opening and closing of the slag release port is controlled by a valve.
[0010] A slag discharge inlet is provided at the top of the carbon dioxide adsorption chamber, and the slag discharge inlet is communicated with the slag release port of the slag insulation chamber. The outlet end of the blast furnace gas booster transmission pipe is inserted into the carbon dioxide adsorption chamber through the bottom of the side wall of the carbon dioxide adsorption chamber, a slag discharge port is provided at the bottom end of the carbon dioxide adsorption chamber, and a high-temperature gas discharge port is provided at the top side of the carbon dioxide adsorption chamber; the carbon dioxide adsorption chamber is a cylindrical structure made of refractory materials, and the angle between the outlet end of the blast furnace gas booster transmission pipe inserted into the side wall of the carbon dioxide adsorption chamber and the tangent of the side wall of the carbon dioxide adsorption chamber is a, wherein a is 5~18°, and the length of the outlet end of the blast furnace gas booster transmission pipe inserted into the carbon dioxide adsorption chamber is 50~100mm.
[0011] The inlet end of the high-temperature gas transmission pipe is connected to the high-temperature gas outlet of the carbon dioxide adsorption chamber, and the outlet end of the high-temperature gas transmission pipe is connected to the high-temperature gas injection pipe and the hydrogen-rich gas injection pipe respectively through a first three-way pipe, and a diverter valve is arranged on the first three-way pipe.
[0012] A circulating gas tuyere is provided on the upper part of the soft melting zone of the side wall of the blast furnace. One end of the high-temperature gas injection pipe is connected to the circulating gas tuyere, and the other end is connected to the high-temperature gas transmission pipe through a first three-way pipeline.
[0013] A second tee is provided on the inlet end of the hydrogen-rich gas injection pipe, a first inlet of the second tee is connected to the high-temperature gas transmission pipe through a pipeline and the first tee, a second inlet of the second tee is connected to the hydrogen storage tank through a pipeline, and the outlet end of the hydrogen-rich gas injection pipe is connected to the blast furnace tuyere.
[0014] The steps include: (1) Mineral charge and coke are added through the top of the blast furnace, wherein the mineral charge is calculated in parts by weight: 65-75 parts by weight of sintered ore (e.g., 66 parts by weight, 68 parts by weight, 69 parts by weight, 70 parts by weight, 71 parts by weight, 72 parts by weight, 73 parts by weight, 73.5 parts by weight, 74 parts by weight, etc.), 10-20 parts by weight of pelletized ore (e.g., 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, etc.), 15 parts by weight, 18 parts by weight, 19 parts by weight, etc.) and 17 to 28 parts by weight of lump ore (for example, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, etc.), the amount of coke added is 290 to 400 kg / t iron; the blast furnace slag is discharged into the slag insulation chamber through the slag ditch of the blast furnace, and then the blast furnace slag is discharged into the carbon dioxide adsorption chamber through the slag release port.
[0015] (2) A portion of the blast furnace gas discharged from the blast furnace top and after dust removal is injected into the carbon dioxide adsorption chamber through the blast furnace gas discharge pipe and the blast furnace gas booster transmission pipe, and the carbon dioxide in the blast furnace gas in the pipe is removed by a carbon dioxide removal component arranged on the blast furnace gas booster transmission pipe. The pressure of the blast furnace gas in the blast furnace gas booster transmission pipe is increased by a gas booster component arranged on the blast furnace gas booster transmission pipe, so that the gas injection speed injected into the carbon dioxide adsorption chamber is 8-15 m / s. 3 / min (e.g. 9m 3 / min、9.8m 3 / min、10.2m 3 / min、11.5m 3 / min、12.3m 3 / min、13.8m 3 / min、14.2m 3 / min, etc.), the blast furnace slag in the carbon dioxide adsorption chamber is stirred and reacted by the injection of blast furnace gas, the carbon dioxide in the blast furnace gas is adsorbed by the blast furnace slag, and the blast furnace gas is heated. The heated blast furnace gas is discharged into the high-temperature gas transmission pipe through the high-temperature gas outlet at the top.
[0016] (3) 30-50% by volume of the high-temperature coal gas (e.g., 32%, 33.5%, 34.2%, 36.8%, 42%, 45.8%, 46.9%, 48%, 49.2%, 49.5%, etc.) is discharged into the high-temperature coal gas injection pipe through the first three-way pipe and the diverter valve, and the remaining high-temperature coal gas is discharged into the hydrogen-rich coal gas injection pipe, which injects the high-temperature coal gas into the high-temperature coal gas injection pipe through the circulating coal gas air injection port.
[0017] (4) hydrogen or a mixture of hydrogen and natural gas is discharged into the second inlet of the second three-way pipe through the hydrogen storage tank, and the hydrogen or a mixture of hydrogen and natural gas is mixed with high-temperature coal gas in the hydrogen-rich coal gas injection pipe, and then injected into the blast furnace through the blast furnace tuyere; the amount of hydrogen or a mixture of hydrogen and natural gas added is 70~100 Nm 3 / tHM (e.g. 75Nm 3 / tHM, 76.5 Nm 3 / tHM, 81 Nm 3 / tHM, 85Nm 3 / tHM, 88 Nm 3 / tHM, 92Nm 3 / tHM, 98 Nm 3 / tHM, etc.). The blast furnace tuyere is the existing blast furnace tuyere.
[0018] (5) After performing step (4) for 1 to 3 hours, the amount of hydrogen or a mixture of hydrogen and natural gas discharged from the hydrogen storage tank is adjusted to 60 to 80 Nm by adjusting the second inlet valve of the second three-way pipe. 3 / tHM (e.g. 61Nm 3 / tHM, 63Nm 3 / tHM, 65Nm 3 / tHM, 68Nm 3 / tHM, 71Nm 3 / tHM, 75Nm 3 / tHM, 76Nm 3 / tHM, etc., which needs to be lower than the amount added in step (4)), after 10 to 30 minutes, readjust the second inlet valve of the second three-way pipe and the hydrogen storage tank, and repeat the hydrogen-rich injection in the manner of step (4).
[0019] Preferably, the distance between the lowest end of the circulating gas tuyere and the topmost position where the soft melting zone meets the side wall of the furnace body is 30-110 cm.
[0020] Preferably, the outlet end of the circulating gas jet is tilted downward, and the inclination angle is 38-50° (for example, 39°, 41°, 42°, 45°, 46°, 48°, etc.) with the horizontal direction.
[0021] As a preference, the gas injection velocity injected into the carbon dioxide adsorption chamber is v, the volume of the carbon dioxide adsorption chamber is V, and 0.8≤V / v(m 3 / min: m 3 )≤5.2 (only the ratio of values, since the unit of v is m 3 / min, the unit of V is m 3 The ratio between the two can be, for example, 0.9, 1, 1.5, 1.8, 2.2, 3, 3.1, 3.8, 4.5, etc.).
[0022] Preferably, in step (2), 30-70% (e.g., 35%, 39%, 45%, 50%, 58%, 62%, 68%, etc.) of the blast furnace gas discharged through the blast furnace gas discharge pipe is discharged into the blast furnace gas booster transmission pipe, and the remaining 30-70% is discharged into the blast furnace gas discharge pipe.
[0023] Preferably, a desulfurization device and a supplementary heat device are further provided on the high-temperature gas transmission pipe. The supplementary heat device is a plasma heating component arranged outside the high-temperature gas transmission pipe. The high-temperature gas in the high-temperature gas transmission pipe is heated to 900-1250°C (for example, 910°C, 925°C, 933°C, 958°C, 980°C, 1015°C, 1018°C, 1120°C, 1158°C, 1168°C, 1208°C, 1211°C, 1225°C, 1238°C, 1241°C, etc.) by the supplementary heat device.
[0024] Preferably, the carbon dioxide removal component is a molecular sieve.
[0025] Preferably, the high-proportion lump ore hydrogen-rich smelting device also includes a dust collector, which is arranged on the blast furnace gas exhaust pipe (the blast furnace gas is first discharged from the blast furnace top through the blast furnace gas exhaust pipe and discharged into the dust collector, and the outlet end of the pipeline where the gas outlet of the dust collector is arranged is the outlet end of the blast furnace gas exhaust pipe) (further preferably, the dust collector is a gravity dust collector and a bag dust collector).
[0026] Preferably, the temperature of the blast furnace gas discharged from the top of the blast furnace in step (2) is 150-380°C.
[0027] Preferably, the temperature of the blast furnace slag in step (1) is 1400-1600°C.
[0028] Preferably, the composition of the blast furnace slag in step (1) is: SiO 2:33.1~36.2wt%, CaO: 31.5~35.0wt%, Fe 2 O 3 :2.3~3.1wt%Al 2 O 3 : 19.6~22.1 wt%, MgO: 1.6~2.8 wt%, and the balance is other impurities.
[0029] Preferably, the hydrogen in step (4) is obtained by electrolyzing water to produce hydrogen after generating electricity using renewable energy including solar energy, wind energy or nuclear energy.
[0030] Preferably, the volume percentage concentration of hydrogen in the mixture of hydrogen and natural gas in step (4) is 60-85%.
[0031] Preferably, the smelting method adopts oxygen-enriched injection (injection is performed at an existing oxygen-enriched injection position). During the oxygen-enriched injection, oxygen-enriched gas with an oxygen content of 90-99v.% is blown into the blast furnace through the tuyere.
[0032] Preferably, before the high-temperature gas containing hydrogen or a mixture of hydrogen and natural gas is sprayed, the volume percentage concentration of carbon dioxide in the blast furnace gas discharged from the furnace top is 6-12%, the volume percentage concentration of carbon monoxide is 28-33%, the volume percentage concentration of hydrogen is 1-4%, the volume percentage concentration of nitrogen is 55-60%, the volume percentage concentration of hydrocarbons is 0.2-0.5%, and the remainder is sulfur dioxide and other impurities. The dust concentration of the blast furnace gas is 10-50g / m 3 .
[0033] The dust particle size is below 500μm, mainly iron, ferrous oxide, aluminum oxide, silicon oxide, magnesium oxide and coke powder.
[0034] As a preferred method, the injection amount of hydrogen in the hydrogen-rich coal gas injection pipe is 50-100m 3 / tIron.
[0035] Preferably, a slag discharge port is also provided at the bottom of the carbon dioxide adsorption chamber.
[0036] The technical effects of the present invention are: (1) The present invention is provided with two sets of tuyere, wherein the circulating gas tuyere provided at the upper end of the side of the soft melting zone is used to strengthen the indirect reduction. The present invention provides a tuyere at this location to inject heated gas, and at the same time indirectly reduces the reaction FeO+CO→Fe+CO 2It is an exothermic reaction, so that in addition to strengthening the indirect reduction, the part above the side of the soft melting zone will also increase the heat from a thermodynamic point of view, thereby strengthening the thermodynamic cycle and kinetic cycle of the gas in the soft melting zone (gas heat increases and strengthens the upward flow). 2 →Fe+H 2 O reaction is an endothermic reaction. If the whole is sprayed at the circulating gas tuyere, it will cause the upper part of the soft melting zone to be overcooled. The present invention sprays the heated blast furnace gas and hydrogen mixture through the normal tuyere of the lower blast furnace, thereby strengthening the hydrogen-rich spraying effect, greatly reducing the addition of carbonaceous raw materials, thereby reducing the generation of carbon dioxide from the source, and reducing the use of carbonaceous raw materials and reducing environmental pollution; at the same time, the present invention sprays different reducing gases at the upper and lower tuyere, and adapts to the amount of hydrogen added, so that the carbon reduction ratio is between 8 and 16%, avoiding the problem of blast furnace running due to excessive carbon reduction, and also avoiding the problem of excessive environmental pollution caused by too little carbon reduction. The amount of hydrogen added is adapted to the different spraying of the two tuyere, and has a close coordination relationship. By reasonably setting the hydrogen-rich spraying, without the need to increase a large amount of coke, under the premise of ensuring the permeability of the soft melting zone, the proportion of natural block ore in the charge is greatly increased, thereby producing better economic benefits from this perspective.
[0037] (2) The present invention allows blast furnace slag to contact blast furnace gas in a specific form, so that carbon dioxide reacts with materials such as calcium oxide in the blast furnace slag to generate carbonates such as calcium carbonate (the blast furnace slag is fully in contact with the air in the slag groove), thereby absorbing carbon dioxide in the blast furnace gas. At the same time, since the temperature of blast furnace slag is generally above 1400°C (and the reaction of carbon dioxide and calcium oxide is also an exothermic reaction), while the temperature of blast furnace gas is generally not more than 500°C, after sufficient contact, not only carbon dioxide in the blast furnace gas is absorbed, but the blast furnace gas is also heated. Although such an idea exists in existing research, the present invention, on this basis, sets the angle between the outlet end of the blast furnace gas booster transmission pipe and the tangent of the side wall of the carbon dioxide adsorption chamber, and other parameters, so that the injected blast furnace gas can fully disturb the blast furnace slag, thereby strengthening the reaction and increasing the contact time and contact area between the gas and the blast furnace slag, thereby greatly strengthening the reaction process and the heat exchange process, and reasonably setting the chamber volume on this basis, so that the gas exists in the chamber for a reasonable length of time under the disturbance. If it is too long (that is, the chamber volume is too large), it will cause a decrease in production efficiency and the slag temperature to drop too low and affect fluidity. If it is too short (that is, the chamber volume is too small), it will lead to insufficient reaction and heat exchange. At the same time, because the present invention coordinates this process with the scheme of staged reuse of blast furnace gas, the blast furnace gas can more fully strengthen the indirect reduction after removing carbon dioxide, and the temperature can also be mixed with hydrogen for hydrogen-rich injection. At the same time, the present invention also provides a plasma heating supplementary heat component outside the tube. Through the plasma heating method, the temperature inside the tube can be controlled very flexibly, so that the heating effect of blast furnace slag heating blast furnace gas is more controllable.
[0038] (3) The present invention sets a specific amount of hydrogen to be added, and such amount of hydrogen to be added is coordinated with the relatively high-calorie high-temperature coal gas sprayed from the upper tuyere. Only after the high-temperature coal gas that strengthens indirect reduction and supplements heat to the upper end of the side of the soft melting zone is sprayed from the upper tuyere, the gas flow is strengthened. Only by adding the hydrogen content of the present invention at this location can the carbon reduction ratio be guaranteed to be between 8 and 16%. Moreover, through the analysis of the furnace top gas, the setting of the hydrogen spray ratio can maximize the utilization rate of hydrogen, so that the hydrogen spray ratio is the optimal ratio setting under the working condition control conditions of the present invention. At the same time, by appropriately reducing the injection amount of hydrogen or a mixture of hydrogen and natural gas for a certain period of time after the injection for a specific period of time, the addition of excessive hydrogen or a mixture of hydrogen and natural gas is avoided, so that the temperature of the tuyere area is reduced and excessive carbonaceous raw materials are replaced. By reducing the injection amount for a certain period of time, the temperature of the hydrogen or the mixture of hydrogen and natural gas in this area and the overall usage of carbonaceous raw materials can fluctuate reasonably (if a relatively low specific amount of hydrogen or hydrogen and natural gas is continuously introduced, it is not easy to change the temperature fluctuation at this location), so that the airflow in this part can form a certain turbulence under a slight change in temperature, thereby strengthening the lateral vector of the airflow to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention is a schematic diagram of a process flow of a high-proportion lump ore hydrogen-enriched smelting method.
[0040] Figure 2 This is a schematic diagram of the connection relationship between the carbon dioxide adsorption chamber and the blast furnace gas pressurization transmission pipe from a top view.
[0041] Wherein: 1-blast furnace, 2-soft melting zone, 3-blast furnace gas discharge pipe, 4-blast furnace gas booster transmission pipe, 5-gas booster component, 6-slag ditch, 7-pipeline for transmitting blast furnace slag, 8-slag insulation chamber, 9-carbon dioxide adsorption chamber, 10-high temperature gas transmission pipe, 11-desulfurization device, 12-heat supplement device, 13-high temperature gas injection pipe, 14-circulating gas tuyere, 15-first three-way pipe, 16-hydrogen storage tank, 17-hydrogen-rich gas injection pipe, 18-tuyere, 19-molecular sieve, 20-blast furnace gas exhaust pipe, 21-dust collector, a-angle between the outlet end of the blast furnace gas booster transmission pipe and the tangent of the side wall of the carbon dioxide adsorption chamber. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described with reference to the embodiments: Example 1
[0043] A steel plant in Hebei Province implemented a high proportion of lump ore hydrogen-rich smelting method. Figure 1 and Figure 2 As shown, using Figure 1 and Figure 2 The high-proportion lump ore hydrogen-rich smelting device shown in the figure includes a blast furnace, a blast furnace gas booster transmission pipe, a carbon dioxide adsorption chamber, a slag insulation chamber, a high-temperature gas transmission pipe, a high-temperature gas injection pipe and a hydrogen-rich gas injection pipe.
[0044] The roof of the blast furnace is provided with a blast furnace gas discharge pipe, on which a dust collector is provided, which are a gravity dust collector and a bag dust collector in sequence, respectively, and the outlet end of the pipe provided with the gas outlet of the dust collector is the outlet end of the blast furnace gas discharge pipe. The outlet end of the blast furnace gas discharge pipe is respectively connected with the inlet end of the blast furnace gas booster transmission pipe and the blast furnace gas dispersing pipe; the blast furnace gas dispersing pipe is connected with an external blast furnace gas treatment device, and a carbon dioxide removal component (a molecular sieve in this embodiment) and a gas booster component are provided on the blast furnace gas booster transmission pipe.
[0045] The slag ditch of the blast furnace is connected to the entrance of the slag insulation chamber through a pipeline, and the slag ditch is in contact with the air to ensure that the calcium oxide in the slag can react with carbon dioxide at high temperature. The slag insulation chamber is arranged above the carbon dioxide adsorption chamber. The slag insulation chamber is a cylindrical cavity made of refractory bricks. A slag release port is opened below the slag insulation chamber, and the opening and closing of the slag release port is controlled by a valve.
[0046] A slag discharge inlet is provided at the top of the carbon dioxide adsorption chamber, and the slag discharge inlet is connected with the slag release port of the slag insulation chamber. The outlet end of the blast furnace gas booster transmission pipe is inserted into the carbon dioxide adsorption chamber through the bottom of the side wall of the carbon dioxide adsorption chamber, and a slag discharge port is provided at the bottom end of the carbon dioxide adsorption chamber, and a high-temperature gas discharge port is provided at the top side of the carbon dioxide adsorption chamber; the carbon dioxide adsorption chamber is a cylindrical structure made of refractory materials, and the angle between the outlet end of the blast furnace gas booster transmission pipe inserted into the side wall of the carbon dioxide adsorption chamber and the tangent of the side wall of the carbon dioxide adsorption chamber is a, wherein a is set to 12° in this embodiment, and the length of the outlet end of the blast furnace gas booster transmission pipe inserted into the carbon dioxide adsorption chamber in this embodiment is 88 mm.
[0047] The inlet end of the high-temperature gas transmission pipe is connected to the high-temperature gas outlet of the carbon dioxide adsorption chamber, and the outlet end of the high-temperature gas transmission pipe is connected to the high-temperature gas injection pipe and the hydrogen-rich gas injection pipe respectively through a first three-way pipe, and a diverter valve is arranged on the first three-way pipe.
[0048] Its Figure 1 As shown, a desulfurization device and a supplementary heat device are also provided on the high-temperature gas transmission pipe. The supplementary heat device is a plasma heating component arranged outside the high-temperature gas transmission pipe. The temperature of the high-temperature gas in the high-temperature gas transmission pipe is heated to 900~1250℃ through the supplementary heat device.
[0049] A circulating gas tuyere is provided on the upper part of the soft melting zone of the side wall of the blast furnace, one end of the high-temperature gas injection pipe is connected to the circulating gas tuyere, and the other end is connected to the high-temperature gas transmission pipe through the first three-way pipeline. Figure 1 The distance between the lowest end of the circulating gas tuyere and the topmost position where the soft melting zone meets the side wall of the furnace body is 30-110 cm (set to 100 cm in this embodiment).
[0050] A second tee is provided on the inlet end of the hydrogen-rich coal gas injection pipe, a first inlet of the second tee is connected to the high-temperature coal gas transmission pipe through a pipeline and the first tee, a second inlet of the second tee is connected to the hydrogen storage tank through a pipeline, and an outlet end of the hydrogen-rich coal gas injection pipe is connected to the blast furnace tuyere. The blast furnace tuyere is the original tuyere of the blast furnace.
[0051] The steps include: (1) Add mineral charge and coke through the top of the blast furnace, where the mineral charge is calculated by weight: 70 parts by weight of sintered ore, 15 parts by weight of pelletized ore and 22 parts by weight of lump ore, and the amount of coke added is 290~320kg / t iron (because the blast furnace works continuously, the amount of coke added is not a specific value and can only be added within a range); discharge the blast furnace slag into the slag insulation chamber through the slag ditch of the blast furnace, and then discharge the blast furnace slag into the carbon dioxide adsorption chamber through the slag release port. The temperature of the discharged blast furnace slag was measured (multiple times) to be 1400~1600℃. The composition of blast furnace slag is: SiO 2 :33.1~36.2wt%, CaO: 31.5~35.0wt%, Fe 2 O 3 :2.3~3.1wt%Al 2 O 3 : 19.6~22.1 wt%, MgO: 1.6~2.8wt%, and the remainder are other impurities.
[0052] (2) The blast furnace gas discharged from the top of the blast furnace is sprayed into the carbon dioxide adsorption chamber after dust removal through the blast furnace gas discharge pipe and the blast furnace gas booster transmission pipe, and the carbon dioxide in the blast furnace gas in the pipe is removed by a carbon dioxide removal component arranged on the blast furnace gas booster transmission pipe. The pressure of the blast furnace gas in the blast furnace gas booster transmission pipe is increased by a gas booster component arranged on the blast furnace gas booster transmission pipe, so that the gas injection speed v injected into the carbon dioxide adsorption chamber is 8~15m 3 / min (the gas injection speed of this embodiment is 12.1m / min as measured by multiple instantaneous measurements 3 / min、9.1m 3 / min, 12.5m3 / min and 11.8m 3 / min), the volume V of the carbon dioxide adsorption chamber in this embodiment is set to 19m 3 The blast furnace slag in the carbon dioxide adsorption chamber is stirred and reacted by the injection of blast furnace gas, the carbon dioxide in the blast furnace gas is adsorbed by the blast furnace slag, and the blast furnace gas is heated. The heated blast furnace gas is discharged into the high-temperature gas transmission pipe through the high-temperature gas outlet at the top. The temperature of the blast furnace gas discharged from the blast furnace top is 150~380℃.
[0053] (3) In this embodiment, 45% of the volume percentage of the high-temperature coal gas is discharged into the high-temperature coal gas injection pipe through the first three-way pipe and the diverter valve, and the remaining high-temperature coal gas is discharged into the hydrogen-rich coal gas injection pipe. The high-temperature coal gas injection pipe injects the high-temperature coal gas through the circulating coal gas injection port.
[0054] (4) hydrogen or a mixture of hydrogen and natural gas is discharged into the second inlet of the second three-way pipe through the hydrogen storage tank, and the hydrogen or a mixture of hydrogen and natural gas is mixed with high-temperature coal gas in the hydrogen-rich coal gas injection pipe, and then injected into the blast furnace through the blast furnace tuyere; the addition amount of hydrogen or a mixture of hydrogen and natural gas is 95Nm 3 / tHM. In order to further improve the environmental friendliness of this embodiment, the hydrogen used is hydrogen obtained by electrolyzing water to produce hydrogen after using renewable energy including solar energy, wind energy or nuclear energy to generate electricity.
[0055] (5) After performing step (4) for 2.5 hours, the amount of hydrogen or a mixture of hydrogen and natural gas discharged from the hydrogen storage tank is adjusted to 78 Nm by adjusting the second inlet valve of the second three-way pipe. 3 / tHM, after 15 minutes, readjust the second inlet valve of the second three-way pipe and the hydrogen storage tank, and repeat the hydrogen-rich injection in the manner of step (4). At the same time, this embodiment is oxygen-rich injection. During oxygen-rich injection, the blast furnace is blown into oxygen-rich gas with an oxygen content of 90-99v.% through the tuyere.
[0056] In order to further strengthen the indirect reduction and fully enable the high-temperature coal gas and the blast furnace air flow to flow in the opposite direction, the outlet end of the circulating gas tuyere described in this embodiment is tilted downward, and the inclination angle is 39° with the horizontal direction (if the angle is too large, the edge heat will be too high, and if the angle is too small, the strengthening effect will not be obvious).
[0057] Through the above implementation of this embodiment, it was measured that the solid fuel ratio decreased from 492 kg / tFe to 408 kg / tFe, the CO utilization rate was maintained above 52%, and the H 2 The utilization rate is 52%. Example 2
[0058] The other configurations of this embodiment are the same as those of the embodiment, except that in step (1), mineral charge and coke are added through the top of the blast furnace, wherein the mineral charge is calculated by weight as follows: 73 parts by weight of sintered ore, 13 parts by weight of pelletized ore, and 19 parts by weight of lump ore, and the amount of coke added is 300-330 kg / t iron.
[0059] Through the above implementation of this embodiment, it was measured that the solid fuel ratio decreased from 492 kg / tFe to 409 kg / tFe, the CO utilization rate was maintained above 53%, and the H 2 The utilization rate is 51%. Comparative Example 1
[0060] This comparative example does not have a circulating gas tuyere. All the heated high-temperature gas is mixed with hydrogen and then injected through the original tuyere of the blast furnace. The other settings are the same as those in Example 1. After a comparative test of the same time as in Example 1, it is found that H 2 The utilization rate is 42%, which is due to the indirect reduction in the upper part of the soft melting zone and insufficient heat, resulting in insufficient hydrogen utilization. Comparative Example 2
[0061] In this comparative example, all the heated high-temperature coal gas and hydrogen are mixed and then sprayed into the blast furnace through the circulating coal gas tuyere. The other settings are the same as those in Example 1. After a comparative test for the same period of time as in Example 1, it is found that the airflow is not smooth. This is because the heat above the soft melting zone itself is insufficient. After the hydrogen is sprayed, the hydrogen reduction reaction absorbs heat, causing the heat to further decrease, thereby causing the problem of the blast furnace running smoothly. Comparative Example 3
[0062] This comparative example adopts a simulation comparison method, and the hydrogen injection rate in step (4) is increased to 135Nm 3 / tHM, it was found that there was a slight disturbance in the smooth operation of the blast furnace. This was because under the setting mode of the present invention, the addition of excessive hydrogen not only caused the temperature of the tuyere area to drop, but also caused excessive replacement of carbonaceous raw materials, thus causing the blast furnace to be disturbed. Comparative Example 4
[0063] In this comparative example, the outlet end of the blast furnace gas booster transmission pipe is inserted into the side wall of the carbon dioxide adsorption chamber, and the angle a between the outlet end and the tangent line of the side wall of the carbon dioxide adsorption chamber is set to 90° (i.e., vertical blowing). Other settings are the same as those in Example 1. After a comparative test for the same time as in Example 1, it is found that the residual amount of carbon dioxide in the high-temperature gas is about twice that of Example 1, and the heating temperature of the high-temperature gas is 850°C, while that of Example 1 is generally above 900°C. This is because the reaction is not sufficient compared with that in Example 1, and the heat exchange is not sufficient. Comparative Example 5
[0064] In this comparative example, 15% of the high-temperature gas by volume is discharged into the high-temperature gas injection pipe through the first three-way pipe and the diverter valve, and the remaining high-temperature gas is discharged into the hydrogen-rich gas injection pipe. The other settings are the same as those in Example 1. After the comparative test for the same time as in Example 1, it is found that H 2 The utilization rate is 48%. Due to the indirect reduction of the upper part of the soft melting zone and the insufficient heat compared with Example 1, the hydrogen utilization rate is insufficient.
[0065] The above embodiments and comparative examples of the present invention are examples and do not limit the protection scope of the technical solution. The lack of comparison of technical features does not mean that there are no outstanding substantive features, but only uses text description to illustrate its setting method.
Claims
1. A method for smelting hydrogen-rich ore using a high proportion of lump ore, characterized in that: The high-proportion lump ore hydrogen-rich smelting device is used, and the high-proportion lump ore hydrogen-rich smelting device includes a blast furnace, a blast furnace gas booster transmission pipe, a carbon dioxide adsorption chamber, a slag insulation chamber, a high-temperature gas transmission pipe, a high-temperature gas injection pipe and a hydrogen-rich gas injection pipe; The roof of the blast furnace is provided with a blast furnace gas discharge pipe, the outlet end of the blast furnace gas discharge pipe is respectively connected with the inlet end of the blast furnace gas booster transmission pipe and the blast furnace gas discharge pipe; the blast furnace gas discharge pipe is connected with an external blast furnace gas treatment device, and a carbon dioxide removal component and a gas booster component are provided on the blast furnace gas booster transmission pipe; The slag channel of the blast furnace is connected to the entrance of the slag insulation chamber through a pipeline. The slag insulation chamber is arranged above the carbon dioxide adsorption chamber. The slag insulation chamber is a square chamber or a cylindrical chamber made of refractory bricks. A slag release port is opened below the slag insulation chamber, and the slag release port is controlled to open and close by a valve. A slag discharge inlet is provided at the top of the carbon dioxide adsorption chamber, and the slag discharge inlet is communicated with the slag release port of the slag insulation chamber. The outlet end of the blast furnace gas booster transmission pipe is inserted into the carbon dioxide adsorption chamber through the bottom of the side wall of the carbon dioxide adsorption chamber, and a slag discharge port is provided at the bottom end of the carbon dioxide adsorption chamber, and a high-temperature gas discharge port is provided at the top side of the carbon dioxide adsorption chamber; the carbon dioxide adsorption chamber is a cylindrical structure made of refractory materials, and the angle between the outlet end of the blast furnace gas booster transmission pipe inserted into the side wall of the carbon dioxide adsorption chamber and the tangent of the side wall of the carbon dioxide adsorption chamber is a, wherein a is 5-18°, and the length of the outlet end of the blast furnace gas booster transmission pipe inserted into the carbon dioxide adsorption chamber is 50-100 mm; The inlet end of the high-temperature gas transmission pipe is connected to the high-temperature gas outlet of the carbon dioxide adsorption chamber, and the outlet end of the high-temperature gas transmission pipe is respectively connected to the high-temperature gas injection pipe and the hydrogen-rich gas injection pipe through a first three-way pipe, and a diverter valve is provided on the first three-way pipe; A circulating gas tuyere is provided on the upper part of the soft melting zone of the side wall of the blast furnace, one end of the high-temperature gas injection pipe is connected to the circulating gas tuyere, and the other end is connected to the high-temperature gas transmission pipe through a first three-way pipeline; A second tee is provided on the inlet end of the hydrogen-rich coal gas injection pipe, a first inlet of the second tee is connected to the high-temperature coal gas transmission pipe through a pipeline and the first tee, a second inlet of the second tee is connected to the hydrogen storage tank through a pipeline, and an outlet end of the hydrogen-rich coal gas injection pipe is connected to the blast furnace tuyere; The steps include: (1) adding mineral charge and coke through the top of a blast furnace, wherein the mineral charge is calculated by weight as follows: 65-75 parts by weight of sintered ore, 15-20 parts by weight of pelletized ore and 17-28 parts by weight of lump ore, and the amount of coke added is 290-400 kg / t iron; discharging the blast furnace slag into a slag insulation chamber through a slag ditch of the blast furnace, and then discharging the blast furnace slag into a carbon dioxide adsorption chamber through a slag discharge port; (2) A portion of the blast furnace gas discharged from the blast furnace top and after dust removal is injected into the carbon dioxide adsorption chamber through the blast furnace gas discharge pipe and the blast furnace gas booster transmission pipe, and the carbon dioxide in the blast furnace gas in the pipe is removed by a carbon dioxide removal component arranged on the blast furnace gas booster transmission pipe. The pressure of the blast furnace gas in the blast furnace gas booster transmission pipe is increased by a gas booster component arranged on the blast furnace gas booster transmission pipe, so that the gas injection speed injected into the carbon dioxide adsorption chamber is 8-15 m / s. 3 / min, the blast furnace slag in the carbon dioxide adsorption chamber is stirred and reacted by the injection of blast furnace gas, the carbon dioxide in the blast furnace gas is adsorbed by the blast furnace slag, and the blast furnace gas is heated, and the heated blast furnace gas is discharged into the high-temperature gas transmission pipe through the high-temperature gas outlet at the top; (3) 30-50% of the volume percentage of the high-temperature coal gas is discharged into the high-temperature coal gas injection pipe through the first three-way pipe and the diverter valve, and the remaining high-temperature coal gas is discharged into the hydrogen-rich coal gas injection pipe. The high-temperature coal gas injection pipe injects the high-temperature coal gas through the circulating coal gas injection port; (4) hydrogen or a mixture of hydrogen and natural gas is discharged into the second inlet of the second three-way pipe through the hydrogen storage tank, and the hydrogen or a mixture of hydrogen and natural gas is mixed with high-temperature coal gas in the hydrogen-rich coal gas injection pipe, and then injected into the blast furnace through the blast furnace tuyere; the amount of hydrogen or a mixture of hydrogen and natural gas added is 70~100 Nm 3 / tHM; (5) After performing step (4) for 1 to 3 hours, the amount of hydrogen or a mixture of hydrogen and natural gas discharged from the hydrogen storage tank is adjusted to 60 to 80 Nm by adjusting the second inlet valve of the second three-way pipe. 3 / tHM, continue for 10 to 30 minutes, readjust the second inlet valve of the second three-way pipe and the hydrogen storage tank, and repeat the hydrogen-rich injection according to step (4).
2. A method for smelting hydrogen using high-proportion lump ore according to claim 1, characterized in that: The distance between the lowest end of the circulating gas tuyere and the topmost position where the soft melting zone meets the side wall of the furnace body is 30-110 cm; The outlet end of the circulating gas jet is tilted downward, and the tilt angle is 38-50° with the horizontal direction; The gas injection velocity injected into the carbon dioxide adsorption chamber is v, and the volume of the carbon dioxide adsorption chamber is V, which satisfies 0.8≤V / v≤5.
2.
3. The method for smelting hydrogen using high-proportion lump ore according to claim 1, characterized in that: In step (2), 30-70% of the blast furnace gas discharged through the blast furnace gas discharge pipe is discharged into the blast furnace gas booster transmission pipe, and the remaining 30-70% is discharged into the blast furnace gas dispersing pipe.
4. The method for smelting hydrogen using high-proportion lump ore according to claim 1, characterized in that: A desulfurization device and a supplementary heat device are also provided on the high-temperature gas transmission pipe. The supplementary heat device is a plasma heating component arranged outside the high-temperature gas transmission pipe. The high-temperature gas in the high-temperature gas transmission pipe is heated to 900-1250°C by the supplementary heat device. The carbon dioxide removal component is a molecular sieve. The high-proportion lump ore hydrogen-rich smelting device also includes a dust collector, which is arranged on the blast furnace gas exhaust pipe.
5. The method for smelting hydrogen using high-proportion lump ore according to claim 1, characterized in that: In step (2), the temperature of the blast furnace gas discharged from the top of the blast furnace is 150-380°C.
6. The method for smelting hydrogen-rich ore using high-proportion lump ore according to claim 1, characterized in that: The temperature of the blast furnace slag in step (1) is 1400-1600°C.
7. The method for smelting hydrogen-rich ore using high-proportion lump ore according to claim 1, characterized in that: The composition of the blast furnace slag in step (1) is: SiO2: 33.1~36.2wt%, CaO: 31.5~35.0wt%, Fe2O3: 2.3~3.1wt%, Al2O3: 19.6~22.1wt%, MgO: 1.6~2.8wt%, and the remainder is other impurities.
8. The method for smelting hydrogen using high-proportion lump ore according to claim 1, characterized in that: The hydrogen in step (4) is obtained by electrolyzing water to produce hydrogen after generating electricity using renewable energy including solar energy, wind energy or nuclear energy.
9. The method for smelting hydrogen-rich ore using high-proportion lump ore according to claim 1, characterized in that: The volume percentage concentration of hydrogen in the mixture of hydrogen and natural gas in step (4) is 60-85%.
10. The method for smelting hydrogen-rich ore using high-proportion lump ore according to claim 1, characterized in that: Oxygen-enriched injection is adopted. During the oxygen-enriched injection, oxygen-enriched gas with an oxygen content of 90-99v.% is blown into the blast furnace through the tuyere.