Method and device for processing 5G hard gold through hard gold powder

Through hard gold powder processing method, using technologies such as medium frequency induction melting furnaces and microalloyization treatment, the problem of low hardness of gold jewelry is solved, and 5G hard gold with higher hardness and toughness is achieved, meeting diversified design needs and extending use life.

CN119040685APending Publication Date: 2024-11-29SHENZHEN JINYAFU JEWELRY MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411152473.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing gold jewelry is prone to deformation and wear due to its low hardness, which limits the diversity and service life of the design styles.

Method used

Through the hard gold powder processing method, the gold is melted by an intermediate frequency induction melting furnace, and the hard gold powder is added for microalloying and continuous extrusion. Combined with the annealing step, the hardness and toughness of the gold are improved to form 5G hard gold.

Benefits of technology

It significantly improves the hardness and corrosion resistance of gold, allowing gold jewelry to have more style designs, reduce deformation and wear, and improves its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004029900000091
    Figure BDA0005004029900000091
  • Figure BDA0005004029900000101
    Figure BDA0005004029900000101
Patent Text Reader

Abstract

The invention relates to the field of gold processing, and particularly discloses a method and device for processing 5G hard gold through hard gold powder. A method for processing 5G hard gold through hard gold powder comprises the following steps of burdening, gold melting, microalloying treatment and continuous extrusion treatment, so that the gold can have richer style design to meet the requirements of people, and manufactured gold accessories are not prone to deformation and abrasion. In the microalloying treatment step, the strength of the gold is improved through the combined action of hard gold powder alloying strengthening and plastic deformation strengthening. In the continuous extrusion treatment step, dislocation motion is generated among metal atoms, along with the increase of deformation, the rapid increase of dislocation density and the interaction of dislocation, a large amount of dislocation entanglement or dislocation accumulation is generated, further movement of dislocation is prevented, rapid increase of deformation resistance is caused, and the strength and hardness of metal are improved. In addition, the device adopts the medium-frequency induction melting furnace, and the medium-frequency induction melting furnace is efficient, environmentally friendly and easy to control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of gold processing, and more specifically, it relates to a method and a device for processing 5G hard gold by using hard gold powder. Background Art

[0002] With the rapid development of China's economy and the improvement of living standards, people's demand for gold jewelry purchase and collection is increasing, and the precious metal industry is also developing rapidly. Gold jewelry has excellent physical and chemical properties, strong corrosion resistance and stable chemical properties, but high-purity gold jewelry has low hardness and is prone to deformation and wear after long-term wearing, which seriously affects the appearance of the jewelry.

[0003] The existing gold jewelry with high hardness traditional craftsmanship is generally formed by reverse molding or rolling technology, and then the surface is calendered to make it round and shiny. Due to the low hardness and high flexibility of gold itself, the pure gold jewelry made by it can only adopt simple and rough styles, and has defects such as easy deformation, easy dirtiness, and easy scratching. Summary of the invention

[0004] In order to increase the hardness of gold and enable gold to have richer styles and designs to meet people's needs, the present application provides a method and a device for processing 5G hard gold using hard gold powder.

[0005] The present application provides a method for processing 5G hard gold by hard gold powder and a device thereof, which adopts the following technical solutions: In the first aspect, the present application provides a method for processing 5G hard gold by hard gold powder, which adopts the following technical solutions: A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: According to weight, weigh 999-1000 parts of gold and 0.1-1 part of hard gold powder and set aside; Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1065-1300℃. After the gold is completely melted, keep it warm for 5-10 minutes. Microalloying treatment: under the protection of inert gas, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2000-2300℃, keep warm and stand for 30-60 minutes to obtain mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 720-840℃ at a rate of 2-3℃ / min, poured into a gold casting, and the gold casting is homogenized at 370-390℃ for 22-26h, and then extruded at 230-270℃ with an extrusion ratio of 21-27.

[0006] By adopting the above technical scheme, after batching, melting gold, microalloying treatment, and continuous extrusion treatment, the hard gold formed has high hardness, so that gold can have richer styles and designs to meet people's needs, and the gold jewelry produced is not easy to deform or wear. In the microalloying treatment step, the strength of gold is improved by the combined action of hard gold powder alloying strengthening and plastic deformation strengthening. The alloy elements in the hard gold powder are dissolved in the matrix metal, and the solute atoms in the replacement solid solution are often evenly distributed. The lattice distortion caused by the different sizes of gold and alloy elements increases the dislocation resistance, causing a certain degree of lattice distortion. Or the alloy elements are often preferentially distributed on the dislocation line, forming an interstitial atomic "air mass", that is, a "Kohlberg air mass", which firmly pins the dislocation and causes strengthening. In the continuous extrusion process, the gold casting is homogenized at 370-390℃ for 22-26h and then extruded at 230-270℃ with an extrusion ratio of 21-27. Dislocation movement occurs between metal atoms. As the deformation increases, the dislocation density increases rapidly. Dislocations interact with each other, resulting in a large number of dislocation entanglements or dislocation accumulations, which prevent further movement of dislocations, causing a sharp increase in deformation resistance, and improving the strength and hardness of the metal. In addition, hard gold powder is dispersed in the matrix, which has the effect of dispersion strengthening.

[0007] Optionally, the following steps are also included: Annealing: After extrusion, homogenization annealing is performed at 165-185℃ for 3-5h.

[0008] By adopting the above technical solution, after extrusion, homogenization annealing is performed at 165-185℃ for 3-5h, which can eliminate the stress generated in microalloying treatment and continuous extrusion treatment, thereby reducing the deformation, cracks and other defects of hard gold caused by stress. Moreover, annealing can repair and eliminate defects such as grain boundaries and dislocations in hard gold, improve the structure and performance of hard gold, and thus improve its toughness and ductility on the basis of improving the hardness of hard gold.

[0009] Optionally, the hard gold powder includes titanium sulfate, tantalum oxide, and niobium carbide.

[0010] By adopting the above technical solution, titanium sulfate, tantalum oxide and niobium carbide work synergistically and exist in the matrix gold in the form of solid solution and second phase particles, thereby refining the gold particles and improving the hardness of hard gold.

[0011] Optionally, the tantalum oxide is tantalum pentoxide.

[0012] By adopting the above technical solution, tantalum pentoxide is well stabilized and has a good synergistic effect with titanium sulfate and niobium carbide.

[0013] Optionally, the hard gold powder also includes rhodium and iridium.

[0014] By adopting the above technical solution, rhodium and iridium can synergistically enhance the effect of solid solution strengthening on the gold matrix, improve the melting point, recrystallization temperature and corrosion resistance of the gold matrix, reduce oxidation and volatilization losses, and the compound formed by rhodium and tantalum oxides can disperse and strengthen the hard gold, increase thermal stability, and iridium and rhodium can also improve the processing performance of hard gold, further enhancing the effect of hard gold powder strengthening the hardness of hard gold. In addition, rhodium and iridium are anti-oxidation and corrosion resistant.

[0015] Optionally, in the hard gold powder, the ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:(0.1-0.6):(0.5-1.2):(0.8-1.5):(0.8-1.5).

[0016] Experiments have found that the ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:(0.1-0.6):(0.5-1.2):(0.8-1.5):(0.8-1.5), which has the best effect of increasing the hardness of gold and can enable gold to have richer styles and designs to meet people's needs.

[0017] Optionally, the inert gas is nitrogen or argon.

[0018] By adopting the above technical solution, nitrogen or argon has high chemical inertness, which can prevent oxygen, hydrogen and other harmful substances from entering the hard gold, reducing the possibility of hard gold being deteriorated by oxygen, hydrogen and other harmful substances.

[0019] Optionally, the inert gas is argon.

[0020] By adopting the above technical solution, argon not only has high chemical inertness but also has high thermal stability, and can effectively protect hard gold even in high temperature environments.

[0021] Optionally, the particle size of the hard gold powder is 30-90 microns.

[0022] By adopting the above technical solution, the particle size of the hard gold powder is 30-90 microns, which can further improve the hardness of the hard gold.

[0023] In a second aspect, the present application provides a device for processing 5G hard gold through hard gold powder, adopting the following technical solution: an apparatus for processing 5G hard gold through hard gold powder as mentioned above, wherein the apparatus adopts a medium frequency induction melting furnace.

[0024] By adopting the above technical solution, firstly, the medium frequency induction melting furnace can melt gold quickly in a short time, thus improving production efficiency. Secondly, the medium frequency induction melting furnace can achieve precise control of the temperature and uniformity of the molten pool by controlling parameters such as current and voltage. Moreover, the medium frequency induction melting furnace does not need to use fuel and oxygen, thus reducing the emission of waste gas and wastewater, which is environmentally friendly. In addition, the operation cost of the medium frequency induction melting furnace is relatively low, and it is easy to maintain and operate.

[0025] In summary, this application has the following beneficial effects: 1. The hard gold formed by the method of the present application has high hardness through the combined effects of alloying strengthening of hard gold powder and plastic deformation strengthening after batching, melting gold, microalloying treatment, continuous extrusion treatment and annealing, so that gold can have richer styles and designs to meet people's needs, and the gold jewelry produced is not easy to deform or wear; 2. In the hard gold powder, titanium sulfate, tantalum oxide, and niobium carbide work together to exist in the matrix gold in the form of solid solution and second phase particles, which refines the gold particles and improves the hardness of the hard gold. Rhodium and iridium can work together to strengthen the gold matrix through solid solution, increase the melting point, recrystallization temperature and corrosion resistance of the gold matrix, and reduce oxidation and volatilization losses. The compound formed by rhodium and tantalum oxides has a dispersion strengthening effect on the hard gold and increases thermal stability. Iridium and rhodium can also improve the processing performance of hard gold, further enhancing the effect of hard gold powder in strengthening the hardness of hard gold. Furthermore, rhodium and iridium are anti-oxidation and corrosion-resistant.

[0026] 3. The device of the present application adopts a medium frequency induction melting furnace, which can melt gold quickly in a short time, thereby improving production efficiency. Secondly, the medium frequency induction melting furnace can achieve precise control of the temperature and uniformity of the molten pool by controlling parameters such as current and voltage. Moreover, the medium frequency induction melting furnace does not require the use of fuel and oxygen, thus reducing the emission of waste gas and wastewater, and is environmentally friendly. In addition, the operating cost of the medium frequency induction melting furnace is relatively low, and it is easy to maintain and operate. DETAILED DESCRIPTION

[0027] The present application is described in further detail below. Example

[0028] Example 1 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 999 parts of gold and 1 part of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide and niobium carbide. The tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide and niobium carbide is 1:0.1:1.2. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The device uses a medium-frequency induction melting furnace with a heating temperature of 1065°C. After the gold is completely melted, keep it warm for 10 minutes. Microalloying treatment: under nitrogen protection, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2000℃, keep warm and stand for 60 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 840℃ at a rate of 2℃ / min, poured into a gold casting, and the gold casting is homogenized at 370℃ for 26h, and then extruded at 230℃ with an extrusion ratio of 27; Annealing: After extrusion, homogenization annealing was performed at 165°C for 5 h.

[0029] Example 2 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 1000 parts of gold and 0.1 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, and niobium carbide. The tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, and niobium carbide is 1:0.6:0.5. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The device uses a medium-frequency induction melting furnace with a heating temperature of 1300°C. After the gold is completely melted, keep it warm for 5 minutes. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2300℃, keep warm and stand for 30 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 720°C at a rate of 3°C / min and poured into a gold casting. The gold casting is homogenized at 390°C for 22 hours and then extruded at 270°C with an extrusion ratio of 21. Annealing: After extrusion, homogenization annealing was performed at 185°C for 3h.

[0030] Example 3 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 999.5 parts of gold and 0.5 parts of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide and niobium carbide. The tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide and niobium carbide is 1:0.3:0.9. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1182.5℃. After the gold is completely melted, keep it warm for 7.5 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under nitrogen protection, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2150℃, keep warm and stand for 45 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 780℃ at a rate of 2.5℃ / min and poured into a gold casting. The gold casting is homogenized at 380℃ for 24h and then extruded at 250℃ with an extrusion ratio of 24. Annealing: After extrusion, homogenization annealing was performed at 175°C for 4 hours.

[0031] Example 4 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 999 parts of gold and 1 part of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium. Tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:0.6:0.5:1.5:0.8. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1065°C. After the gold is completely melted, keep it warm for 10 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under nitrogen protection, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2000℃, keep warm and stand for 60 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 720°C at a rate of 3°C / min and poured into a gold casting. The gold casting is homogenized at 390°C for 22 hours and then extruded at 270°C with an extrusion ratio of 21. Annealing: After extrusion, homogenization annealing was performed at 165°C for 3 h.

[0032] Example 5 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 1000 parts of gold and 0.1 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, niobium carbide, rhodium, and iridium. Tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium, and iridium is 1:0.35:0.85:1.2:1.3; Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1300℃. After the gold is completely melted, keep it warm for 5 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2300℃, keep warm and stand for 30 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 840℃ at a rate of 2℃ / min, poured into a gold casting, and the gold casting is homogenized at 370℃ for 26h, and then extruded at 230℃ with an extrusion ratio of 27; Annealing: After extrusion, homogenization annealing was performed at 185°C for 5 h.

[0033] Example 6 A method for processing 5G hard gold by hard gold powder comprises the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium. Tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:0.1:1.2:0.8:1.5. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0034] Comparative Example Comparative Example 1 A method for processing gold comprises the following steps: Ingredients: Weigh 999.3 parts of gold by weight and set aside; Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Continuous extrusion treatment: The gold melt obtained in the gold melting step is cooled to 760°C at a rate of 2.6°C / min, and poured into a gold casting. The gold casting is homogenized at 385°C for 25 hours, and then extruded at 260°C with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0035] Comparative Example 2 A method for processing gold comprises the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes rhodium and iridium. The ratio of rhodium to iridium is 0.8:1.5. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0036] Comparative Example 3 A method for processing gold, comprising the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate and tantalum oxide. The tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate to tantalum oxide is 1:0.1. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0037] Comparative Example 4 A method for processing gold, comprising the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes tantalum oxide and niobium carbide. The tantalum oxide is tantalum pentoxide. The ratio of tantalum oxide to niobium carbide is 0.1:1.2. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0038] Comparative Example 5 A method for processing gold, comprising the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight, and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate and niobium carbide. The ratio of titanium sulfate to niobium carbide is 1:1.2. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Annealing: After extrusion, homogenization annealing was performed at 180°C for 3.5h.

[0039] Comparative Example 6 A method for processing gold, comprising the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium. Tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:0.1:1.2:0.8:1.5. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 760℃ at a rate of 2.6℃ / min and poured into a gold casting. The gold casting is homogenized at 385℃ for 25h and then extruded at 260℃ with an extrusion ratio of 22. Cooling: After extrusion, the gold casting is left to cool to room temperature.

[0040] Comparative Example 7 A method for processing gold, comprising the following steps: Ingredients: weigh 999.3 parts of gold and 0.7 parts of hard gold powder by weight and set aside. The particle size of the hard gold powder is 30-90 microns. The hard gold powder includes titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium. Tantalum oxide is tantalum pentoxide. The ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:0.1:1.2:0.8:1.5. Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1090°C. After the gold is completely melted, keep it warm for 9 minutes. The device uses a medium frequency induction melting furnace. Microalloying treatment: under the protection of argon, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2250℃, keep warm and stand for 35 minutes to obtain a mixed gold melt; Casting: Cool the mixed gold melt to 760°C at a rate of 2.6°C / min and cast it into a gold casting; Cooling: After casting, the gold casting is left to cool to room temperature.

[0041] Comparative Example 8 Commercially available 3D gold.

[0042] Comparative Example 9 Commercially available 5D gold.

[0043] Performance Testing The hard gold prepared by the method of processing 5G hard gold by hard gold powder in Examples 1-6, the gold prepared by the method of processing gold in Comparative Examples 1-7, and the gold in Comparative Examples 8-9 were tested for hardness and gold content.

[0044] Hardness: Refer to GB / T4340-2009 "Vickers hardness test for metal materials" for testing.

[0045] Gold content: Refer to GB / T9288-2019 "Determination of gold content of gold alloy jewelry - ash blowing method (fire assay method)" for testing to determine whether the gold content is greater than 99%.

[0046] The test results are as follows: Table 1 Test results Comparing Examples 1-6 with Comparative Example 1, the hardness of Examples 1-6 is higher than 120HV, and the gold content is greater than 99%, which meets the requirements of pure gold; although the gold content of Comparative Example 1 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 1 is significantly lower than that of Examples 1-6, indicating that the hard gold formed by the combined effects of hard gold powder alloying strengthening and plastic deformation strengthening in the present application has high hardness, so that gold can have richer styles and designs to meet people's needs, and the gold jewelry produced is not easy to deform or wear.

[0047] Comparing Examples 1-6 with Comparative Example 2, although the gold content of Comparative Example 2 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 2 is significantly lower than that of Examples 1-6, indicating that titanium sulfate, tantalum oxide, and niobium carbide play an important role in improving the hardness of hard gold.

[0048] Comparing Examples 1-6 with Comparative Example 3, although the gold content of Comparative Example 3 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 3 is significantly lower than that of Examples 1-6, indicating that niobium carbide plays an important role in improving the hardness of hard gold.

[0049] Comparing Examples 1-6 with Comparative Example 4, although the gold content of Comparative Example 3 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 3 is significantly lower than that of Examples 1-6, indicating that titanium sulfate plays an important role in improving the hardness of hard gold.

[0050] Comparing Examples 1-6 with Comparative Example 5, although the gold content of Comparative Example 3 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 3 is significantly lower than that of Examples 1-6, indicating that tantalum oxide plays an important role in improving the hardness of hard gold.

[0051] In summary, titanium sulfate, tantalum oxide, and niobium carbide synergistically increase the hardness of hard gold.

[0052] Comparing Examples 1-6 with Comparative Example 6, although the gold content of Comparative Example 6 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 6 is significantly lower than that of Examples 1-6, indicating that the annealing step plays an important role in enhancing the hardness of gold.

[0053] Comparing Examples 1-6 with Comparative Example 7, although the gold content of Comparative Example 7 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 7 is significantly lower than that of Examples 1-6, indicating that the continuous extrusion treatment step plays an important role in enhancing the hardness of gold.

[0054] Comparing Examples 1-6 with Comparative Example 8, although the gold content of Comparative Example 8 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 8 is significantly lower than that of Examples 1-6, indicating that the hard gold of the present application has significantly improved hardness compared to commercially available 3D gold.

[0055] Comparing Examples 1-6 with Comparative Example 9, although the gold content of Comparative Example 9 is also greater than 99%, which meets the requirements of pure gold, the hardness of Comparative Example 9 is significantly lower than that of Examples 1-6, indicating that the hard gold of the present application has significantly improved hardness compared with commercially available 5D gold.

[0056] The above specific embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the present application without any creative contribution as needed, but all modifications shall be included in the scope of protection of the present application.

Claims

1. A method for processing 5G hard gold by hard gold powder, It is characterized in that The following steps are included: Ingredients: According to weight, weigh 999-1000 parts of gold and 0.1-1 part of hard gold powder and set aside; Melting gold: Place the gold in a device that processes 5G hard gold through hard gold powder and heat it to melt. The heating temperature is 1065-1300℃. After the gold is completely melted, keep it warm for 5-10 minutes. Microalloying treatment: under the protection of inert gas, add hard gold powder to the molten gold liquid, stir the molten gold liquid to make the hard gold powder and the gold liquid evenly mixed, continue to heat to 2000-2300℃, keep warm and stand for 30-60 minutes to obtain mixed gold melt; Continuous extrusion treatment: The mixed gold melt is cooled to 720-840℃ at a rate of 2-3℃ / min, poured into a gold casting, and the gold casting is homogenized at 370-390℃ for 22-26h, and then extruded at 230-270℃ with an extrusion ratio of 21-27.

2. A method for processing 5G hard gold by hard gold powder according to claim 1, Features: The following steps are also included: Annealing: After extrusion, homogenization annealing is performed at 165-185℃ for 3-5h.

3. A method for processing 5G hard gold by hard gold powder according to claim 1, Features: The hard gold powder includes titanium sulfate, tantalum oxide and niobium carbide.

4. A method for processing 5G hard gold by hard gold powder according to claim 1, Features: The tantalum oxide is tantalum pentoxide.

5. A method for processing 5G hard gold by hard gold powder according to claim 3, Features: The hard gold powder also includes rhodium and iridium.

6. A method for processing 5G hard gold by hard gold powder according to claim 5, Features: In the hard gold powder, the ratio of titanium sulfate, tantalum oxide, niobium carbide, rhodium and iridium is 1:(0.1-0.6):(0.5-1.2):(0.8-1.5):(0.8-1.5).

7. A method for processing 5G hard gold by hard gold powder according to claim 1, Features: The inert gas is nitrogen or argon.

8. A method for processing 5G hard gold by hard gold powder according to claim 7, Features: The inert gas used is argon.

9. A method for processing 5G hard gold by hard gold powder according to claim 1, Features: The particle size of the hard gold powder is 30-90 microns.

10. A device for processing 5G hard gold by hard gold powder according to any one of claims 1 to 9, Features: The device adopts a medium frequency induction melting furnace.