Aluminum alloy automobile steering knuckle and extrusion casting production method thereof
By optimizing the composition and deep purification technology of aluminum alloy, combined with powder refining and gas refining, the problem of insufficient strength and plasticity of aluminum alloy automobile steering joints is solved, and efficient and low-cost aluminum alloy automobile steering joint production is achieved, satisfying the lightweight automobile The demand for quantitative development.
Patent Information
- Application Number
- CN202410999929.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
AI Technical Summary
The strength and hardness of existing aluminum alloy automobile steering knuckles are relatively low, and the plasticity is poor, making it difficult to meet the development needs of automobile lightweight. At the same time, the production cost of forging methods is relatively high. Adding reinforcement elements such as Cu improves mechanical properties but reduces plasticity. Increased production costs.
The deformation aluminum alloy is used for extrusion casting. By optimizing the composition of aluminum alloy and deeply purifying the aluminum alloy liquid, the content of Mg, Si, Cu, Cr, Mn, Ti, Fe is controlled, and the powdering refining and mixed gas refining technology are combined. Perform solid solution and aging treatment to obtain high-strength aluminum alloy automotive steering knuckle.
It significantly improves the tensile strength, yield strength and plasticity of aluminum alloy car steering joints, reduces production costs, avoids the high cost of Cu elements, and shortens the solid solution and aging treatment time, and improves production efficiency.
Smart Images

Figure CN119040712A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy automobile parts forming, and in particular relates to an aluminum alloy automobile steering knuckle and an extrusion casting production method thereof. Background Art
[0002] Aluminum alloy steering knuckle is a key component of automobile steering system, which undertakes the important task of transmitting steering torque. Its safety and reliability directly affect the driving safety of automobile and the life safety of passengers. With the development of automobile lightweight, the mechanical properties of aluminum alloy steering knuckle are required to be higher and higher, requiring both higher strength and higher plasticity to meet the design and manufacturing requirements of aluminum alloy steering knuckle lightweight and improve the safety and reliability of automobile driving.
[0003] The Chinese patent with publication number CN113684402A discloses a method for preparing a rare earth aluminum alloy steering knuckle with good toughness. The steering knuckle is composed of the following components in weight percentage: Si 6.8-8%, Mg 0.3-0.5%, Cu0.1-2%, Ti 0.12-0.25%, rare earth alloy ≤10%, Fe ≤0.12%, unavoidable impurities ≤0.10%, and the rest is Al. The preparation method includes batching, preheating, heating and melting, first refining, standing, adding rare earth alloy, stirring, heat preservation, second refining, heat preservation and standing, and casting.
[0004] The Chinese patent with publication number CN111842800A discloses a method for casting aluminum alloy steering knuckle with aluminum alloy ingot, including melting aluminum alloy ingot, casting, cutting off flash, sawing off gate, pre-drilling center hole, X-ray inspection, heat treatment. The aluminum alloy steering knuckle is composed of the following components in mass percentage: Si 6.6-7.4%, Fe≤0.12, Cu≤0.02, Mn≤0.05, Mg 0.3-0.45%, Zn≤0.05, Ni≤0.05, Pb≤0.03, Sn≤0.01, Ti0.1-0.15%, Sb≤0.005, and the rest is Al. The mechanical properties of the aluminum alloy steering knuckle are relatively low, with yield strength ≥260Mpa, tensile strength ≥320Mpa, elongation ≥8%, and Brinell hardness ≥90HB.
[0005] The Chinese patent with publication number CN106917014A discloses a car aluminum alloy steering knuckle and its extrusion casting method. The aluminum alloy steering knuckle is composed of the following components: Si 3-6%, Cu 3.5-4.5%, Mg 0.15-0.40%, Ti 0.05-0.30%, RE 0-0.5%, and the rest is Al. The extrusion casting method includes the following steps: heating and melting, adding Al-5Ti-B refiner, refining through argon, preheating the mold, closing the mold and pouring, extrusion casting, and heat treatment. The tensile strength of the aluminum alloy steering knuckle is greater than 430MPa, the yield strength is greater than 328MPa, the elongation is greater than 9.6%, and the hardness is greater than HB135. Although the mechanical properties of the aluminum alloy steering knuckle are relatively high, it contains a large amount of Cu element, which is not conducive to reducing production costs.
[0006] The Chinese patent with publication number CN107955893A discloses a forging method for an aluminum alloy steering knuckle, including aluminum alloy bar material cutting, heating, roughing, secondary heating, die forging, water cooling, trimming, aging, inspection and packaging. The aluminum alloy bar material is a 6082 round bar, which has the following components: Si 0.7-1.3%, Mg 0.6-1.2%, Mn 0.4-1.0%, Fe≤0.5%, Zn≤0.2%, Cr≤0.25%, Cu≤0.10%, Ti≤0.10%, and the rest is Al. The yield strength of the steering knuckle is greater than 310MPa, the tensile strength is greater than 335MPa, and the elongation is greater than 12%. Although the mechanical properties of the forged aluminum alloy steering knuckle are relatively high, the forging process is long and the process is multi-step, so the production cost is also relatively high.
[0007] Based on the results of literature inspection and production practice experience, the existing aluminum alloy automobile steering knuckles and their forming methods still have one or more of the following problems: (1) The existing cast aluminum alloy automobile steering knuckles are mainly cast aluminum silicon alloys, which generally have low strength and hardness and poor plasticity, and are difficult to meet the development needs of lightweight automobiles. (2) Although forged aluminum alloy automobile steering knuckles have high strength, hardness and plasticity, the production cost is high, which is not conducive to the promotion and application of forged aluminum alloy automobile steering knuckles. (3) Although the strength and hardness of aluminum alloy automobile steering knuckles can be improved by adding strengthening elements such as Cu, the plasticity of aluminum alloy automobile steering knuckles will be reduced, while the production cost will be increased, which is not conducive to the promotion and application of aluminum alloy automobile steering knuckles. Therefore, the existing aluminum alloy automobile steering knuckles and their forming methods still need to be improved and developed. Summary of the invention
[0008] In view of the problems and shortcomings mentioned in the background technology, the purpose of the present invention is to provide an aluminum alloy automobile steering knuckle and an extrusion casting production method thereof, which can improve the strength, hardness and plasticity of the aluminum alloy automobile steering knuckle by optimizing the component composition of the aluminum alloy and deeply purifying the aluminum alloy liquid, obtain a high-strength and tough aluminum alloy automobile steering knuckle, reduce the production cost of the aluminum alloy automobile steering knuckle, meet the needs of automobile lightweight development, improve the safety and reliability of automobile driving, and solve the problems mentioned in the background technology.
[0009] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows:
[0010] The first aspect of the present invention provides an aluminum alloy automobile steering knuckle, which is characterized in that the aluminum alloy automobile steering knuckle is composed of the following components in mass percentage: Mg 0.98-1.02%, Si 0.73-0.78%, Cu 0.21-0.26%, Cr0.18-0.22%, Mn 0.1-0.15%, Ti 0.015-0.02%, Fe≤0.15%, and the balance is Al and other inevitable impurities, the individual content of other impurities is ≤0.05%, and the total content of other impurities is ≤0.15%.
[0011] Existing aluminum alloy automobile steering knuckles are mainly formed by casting aluminum silicon alloy. Although the cast aluminum silicon alloy has good casting fluidity and is easy to cast, the cast aluminum silicon alloy generally has the problems of low strength and poor plasticity, which seriously restricts the high performance and light weight of aluminum alloy automobile steering knuckles. The present invention breaks through the traditional concept and uses a deformed aluminum alloy to extrude and cast an aluminum alloy automobile steering knuckle. Since the deformed aluminum alloy has higher strength and plasticity than the cast aluminum silicon alloy, it is conducive to extrusion casting of high-strength and high-plasticity aluminum alloy automobile steering knuckles.
[0012] Among them, Mg, Si, and Cu are the main strengthening elements of aluminum alloy automobile steering knuckles. Mg and Si can not only improve the strength of aluminum alloy automobile steering knuckles through solid solution strengthening, but also precipitate Mg through aging. 2 Si phase further enhances the strength of aluminum alloy automobile steering knuckle. Cu can also improve the strength of aluminum alloy automobile steering knuckle through solid solution strengthening, and can also precipitate CuAl 2 The phase further enhances the strength of the aluminum alloy automobile steering knuckle. The higher the content of Mg, Si, and Cu, the higher the strength of the aluminum alloy automobile steering knuckle, but it will also cause a decrease in plasticity. In order to obtain an aluminum alloy automobile steering knuckle with both high strength and high plasticity, the content of Mg, Si, and Cu must be strictly limited.
[0013] Cr and Mn can form MnAl in aluminum alloy automobile steering knuckles. 6 CrAl 7Dispersed particles enhance the strength of aluminum alloy automobile steering knuckles, and also refine grains, inhibit grain growth, and increase recrystallization temperature. The higher the Cr and Mn content, the higher the strength of the aluminum alloy automobile steering knuckles, but it will also cause a decrease in plasticity. Therefore, the Cr and Mn content must also be strictly controlled.
[0014] The Ti element is added to the aluminum alloy liquid in the form of aluminum-titanium-boron alloy or aluminum-titanium-carbon alloy refiner. Its main function is to refine the grain structure of the aluminum alloy automobile steering knuckle and improve the uniformity of the organizational composition and mechanical properties of the aluminum alloy automobile steering knuckle. The Ti content cannot be too low, otherwise the grain refinement effect is not obvious. The Ti content does not need to be too high either. Too high a Ti content can neither enhance the grain refinement effect nor increase the production cost.
[0015] Fe is an inevitable impurity element in aluminum alloys. It is usually present in the form of FeAl 3 , Fe 2 SiAl 9 The presence of coarse needle-like or flaky iron-rich phases will split the aluminum matrix of the aluminum alloy automobile steering knuckle, destroy the continuity of the organization, cause local stress concentration, become the crack source and crack extension direction of the aluminum alloy automobile steering knuckle fracture, and reduce the strength and plasticity of the aluminum alloy automobile steering knuckle. Therefore, the content of impurity element Fe must also be strictly controlled.
[0016] The second aspect of the present invention provides an extrusion casting production method for an aluminum alloy automobile steering knuckle, which is characterized by comprising the following steps in sequence:
[0017] Step 1: Smelting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy automobile steering knuckle;
[0018] Step 2: using inert gas and powder refining agent to spray and refine the aluminum alloy liquid to remove slag and hydrogen;
[0019] Step 3: Adding a refiner to refine and modify the aluminum alloy liquid;
[0020] Step 4: using mixed gas to spray and refine the aluminum alloy liquid to remove hydrogen and slag;
[0021] Step 5: Extrusion casting the aluminum alloy liquid into an aluminum alloy automobile steering knuckle blank;
[0022] Step 6: Cut off the flash and gate of the aluminum alloy automobile steering knuckle blank;
[0023] Step 7: subjecting the aluminum alloy automobile steering knuckle to solid solution and aging treatment;
[0024] Step eight: performing surface sandblasting treatment on the aluminum alloy automobile steering knuckle to obtain the aluminum alloy automobile steering knuckle.
[0025] Preferably, the inert gas in step 2 is argon with a purity of ≥99.99%, the amount of the powder refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during the spray refining is 700-720°C, and the spray refining time is 15-20 minutes.
[0026] The spray refining adopts a powder spraying tank and a stainless steel pipe, uses inert gas argon as a carrier, sprays the powder refining agent into the aluminum alloy liquid, makes the powder refining agent contact and react with the aluminum alloy liquid, and then takes the inclusions and hydrogen in the aluminum alloy liquid out of the aluminum alloy liquid, so as to achieve the purpose of removing slag and hydrogen.
[0027] The deslagging and dehydrogenation effects of spray refining are related to the purity of the inert gas, the amount of powder refining agent, the quality of the powder refining agent, the temperature of the aluminum alloy liquid and the spray refining time. The higher the purity of the inert gas argon, the better. In order to ensure the deslagging and dehydrogenation effects of spray refining and avoid the introduction of water vapor to cause the aluminum alloy liquid to absorb hydrogen, argon with a purity of ≥99.99% is preferred.
[0028] The greater the amount of powder refining agent used, the longer the spray refining time, and the better the slag removal and hydrogen removal effect of the spray refining, but the production cost will increase accordingly. However, if the temperature of the aluminum alloy liquid is too high or the spray refining time is too long, the oxidation and burning of the aluminum alloy liquid will also increase. Comprehensively assessing the slag removal and hydrogen removal effect and production cost of spray refining, preferably, the amount of powder refining agent used is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during the spray refining is 700-720°C, and the spray refining time is 15-20 minutes. After the spray refining is completed, after removing the scum on the surface of the aluminum alloy liquid, a covering agent should be sprinkled on the surface of the aluminum alloy liquid in time to avoid oxidation and burning of the aluminum alloy liquid and hydrogen absorption. After sprinkling the covering agent, the aluminum alloy liquid needs to be left to stand for a period of time so that the inclusions and bubbles in the aluminum alloy liquid float out. The standing time of the aluminum alloy liquid cannot be less than 30 minutes. As a preferred embodiment, the standing time of the aluminum alloy liquid is 30-40 minutes.
[0029] Preferably, the powder refining agent in step 2 is composed of the following components in percentage by mass: NaCl 35.12%, NaF 19.84%, TiCl 3 16.51%, SrSO 4 10.06%, KPO 3 11.45%, Na 2 B 4 O 7 7.02%.
[0030] The deslagging and dehydrogenation effects of powder refining are closely related to the composition of the powder refining agent. Existing powder refining agents are mainly obtained by crushing and mixing fluoride salts and chloride salts. The deslagging and dehydrogenation efficiency of powder refining agents is low, and there are also problems such as large irritating smoke emissions and single functions, which are difficult to meet the production needs of high-cleanliness and high-performance aluminum alloys.
[0031] In order to improve the deslagging and dehydrogenation effect of powder spray refining, the present invention has developed a highly efficient and environmentally friendly multifunctional powder refining agent, in which NaCl reacts with aluminum liquid to generate AlCl with a boiling point of only 180°C. 3 , AlCl 3 During the floating process, the bubbles absorb and capture inclusions and hydrogen that escape from the molten aluminum, thereby removing slag and hydrogen.
[0032] NaF molten salt can destroy the alumina film, dissolve inclusions such as alumina into the molten salt, increase the surface tension between the inclusions and the aluminum liquid, promote the separation of inclusions such as alumina from the aluminum liquid, and enhance the slag removal function of the powder refining agent.
[0033] TiCl 3 Reacts with aluminum liquid to form AlCl 3 Bubbles, AlCl 3 During the floating process, the bubbles absorb and capture inclusions and hydrogen in the aluminum liquid, enhancing the slag and hydrogen removal capabilities of the powder refining agent. The Ti element obtained by the reaction enters the aluminum liquid, which can refine the α-Al grains of the aluminum alloy automobile steering knuckle and improve the uniformity of the aluminum alloy automobile steering knuckle.
[0034] SrSO 4 Reacts with aluminum liquid to generate SO 2 Bubbles, SO 2 During the floating process, the bubbles can absorb and capture inclusions and hydrogen in the aluminum liquid, enhancing the slag and hydrogen removal capabilities of the powder refining agent. The Sr element obtained by the reaction enters the aluminum liquid, which can refine the modified eutectic Si phase and improve the strength and plasticity of the aluminum alloy automobile steering knuckle.
[0035] KPO 3 The P element generated by reacting with aluminum liquid enters the aluminum liquid, which can refine the modified primary Si phase, not only improving the strength and plasticity of the aluminum alloy automobile steering knuckle, but also enhancing the wear resistance of the aluminum alloy automobile steering knuckle.
[0036] Na 2 B 4 O 7 By reacting with aluminum liquid to generate element B which enters into the aluminum liquid, the coarse Fe-rich phase can be refined and modified, eliminating the harm of the coarse Fe-rich phase to the strength and plasticity of aluminum alloy automobile steering knuckle, thereby improving the strength and plasticity of aluminum alloy automobile steering knuckle.
[0037] Preferably, the preparation method of the powder refining agent in step 2 comprises the following steps in sequence: (1) selecting NaCl, NaF, TiCl with a purity of ≥ 99.8% according to the composition and mass percentage of the powder refining agent; 3 、SrSO 4 , KPO 3 、Na 2 B 4 O 7 The steps of: (1) preparing ingredients for the raw materials; (2) adding the ingredients into water at a temperature of 70° C. and stirring to dissolve the ingredients into an aqueous solution, wherein the mass ratio of water to the ingredients is 1.2, and then heating the aqueous solution to 100° C. to evaporate the aqueous solution to obtain solid crystals; and (3) crushing the solid crystals into powders with a particle size of less than 2 mm, and drying and dehydrating the powders at 160° C. for 4 hours to obtain the powder refining agent.
[0038] The deslagging and dehydrogenation effects of powder refining agents are closely related to their preparation methods. The conventional preparation method of existing powder refining agents is to mechanically crush chloride salts and fluoride salts and then directly mix them to obtain powder refining agents. The powder refining agents prepared by this method have independent components, a high melting point, and low degassing and deslagging efficiency. The present invention breaks through tradition and adopts a solution evaporation method to prepare powder refining agents. Through solution evaporation, the components are re-solidified and recrystallized to form a eutectic with a lower melting point. For example, the melting point of NaCl is usually 801°C, and the melting point of NaF is usually 993°C. When the two form a NaCl·NaF eutectic, the melting point drops to 698°C, thereby greatly reducing the melting point of the powder refining agent, making the powder refining agent easier to dissolve in aluminum alloy liquid, and enhancing the deslagging and dehydrogenation effects of the powder refining agent.
[0039] Preferably, the refiner in step three is an Al-5Ti-1B alloy rod or an Al-5Ti-0.2C alloy rod, and the amount of the refiner added is 0.3-0.4% of the weight of the aluminum alloy liquid.
[0040] The purpose of adding refiners is to refine the α-Al grains and improve the fluidity and uniformity of the aluminum alloy liquid. If refiners are not added for refinement and modification, coarse dendritic α-Al grains will be formed during the solidification of the aluminum alloy liquid, which will not only reduce the fluidity of the aluminum alloy liquid and increase the difficulty of filling, but also cause component segregation and uneven structure inside the aluminum alloy. The grain refiner can be an Al-5Ti-1B alloy rod or an Al-5Ti-0.2C alloy rod. The addition amount cannot be less than 0.3%, otherwise the grain refinement effect will not be obvious. The addition amount does not need to exceed 0.4%. Adding more than 0.4% will not significantly increase the grain refinement effect, but will increase production costs.
[0041] Preferably, the amount of the mixed gas in step 4 is 2-3 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is (0.3-0.5)×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.
[0042] After powder spray refining, the gas slag content of aluminum alloy liquid has been greatly reduced, but the aluminum alloy liquid still contains gas slag, because the powder refining agent refining process re-introduces inclusions such as chloride salts and fluoride salts. In addition, although the powder refining agent spray refining also has a dehydrogenation effect, the dehydrogenation effect is limited, because the powder refining agent inevitably contains water, which will also be introduced during the spray refining and dehydrogenation, causing the aluminum alloy liquid to absorb hydrogen again, so that the dehydrogenation of the powder refining agent spray refining is always in a dynamic equilibrium process. It is difficult for the powder refining agent spray refining to reduce the hydrogen content of the aluminum alloy liquid to below 0.2ml / 100gAl. Therefore, in order to obtain a highly clean aluminum alloy liquid, gas refining, dehydrogenation and deslag removal must also be carried out.
[0043] The mixed gas blowing refining adopts a stainless steel pipe or a degasser to blow the mixed gas into the aluminum alloy liquid, so that the mixed gas forms fine bubbles and contacts and reacts with the aluminum alloy liquid, and the hydrogen and inclusions in the aluminum alloy liquid are brought out of the liquid surface by the bubbles floating, so as to achieve the purpose of slag removal and hydrogen removal.
[0044] The dehydrogenation and deslagging effect of mixed gas spray refining is related to the amount of mixed gas, the temperature of aluminum alloy liquid and the spray refining time. The greater the amount of mixed gas used and the longer the spray refining time, the better the deslagging and dehydrogenation effect of spray refining, but the production cost will increase accordingly. However, if the temperature of aluminum alloy liquid is too high or the spray refining time is too long, the oxidation and burning of aluminum alloy liquid will also increase. Preferably, the amount of mixed gas used is 2-3 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is (0.3-0.5)×10 5 Pa, the temperature of the aluminum alloy liquid during the spray refining is 700-720℃, and the spray refining time is 10-15 minutes. After the spray refining is completed, after the scum on the surface of the aluminum alloy liquid is scraped off, a covering agent should be sprinkled on the surface of the aluminum alloy liquid in time to avoid oxidation, burning and hydrogen absorption of the aluminum alloy liquid. After sprinkling the covering agent, the aluminum alloy liquid needs to be left to stand for a period of time so that the bubbles in the aluminum alloy liquid float out. The standing time of the aluminum alloy liquid cannot be less than 20 minutes. As a preferred embodiment, the standing time of the aluminum alloy liquid is 20-30 minutes.
[0045] Preferably, the mixed gas in step 4 is composed of argon gas with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide, the volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, and the volume percentage of carbon monoxide is 3-5%.
[0046] In the existing gas injection refining technology, inert gas nitrogen or argon, or a mixture of inert gas and chlorine, is usually injected into the aluminum alloy liquid. Since nitrogen, argon and chlorine have small relative molecular weights and low gas densities, the relative molecular mass of nitrogen is 28.01 and the density is 1.25 kg / m 3 The relative molecular mass of argon is 39.94 and the density is 1.78 kg / m 3 The relative molecular mass of chlorine is 70.91 and the density is 3.21kg / m 3 . This causes the bubbles to float faster in the aluminum alloy liquid, and the contact time between the bubbles and the aluminum alloy liquid is shorter, which greatly affects the dehydrogenation and deslagging effect of gas injection refining. In addition, although the relative density of chlorine is relatively large, chlorine is a toxic gas with a strong pungent odor, which will not only seriously corrode the smelting furnace and smelting tools, but also cause serious environmental pollution.
[0047] Aiming at the problems and shortcomings of the existing gas injection refining technology, in order to improve the dehydrogenation and slag removal effect of gas injection refining, the present invention injects a mixed gas consisting of argon with a purity of ≥99.99%, sulfur hexafluoride with a purity of ≥99.99% and carbon monoxide with a purity of ≥99.99% into the aluminum alloy liquid, wherein sulfur hexafluoride is a high-density, high-stability gas, and sulfur hexafluoride is non-toxic, non-combustible and non-corrosive. The relative molecular mass of sulfur hexafluoride is 146.05 and the density is 6.5kg / m 3 , adding 9-11% by volume of sulfur hexafluoride to the mixed gas can significantly slow down the floating speed of bubbles in the aluminum alloy liquid, increase the contact time between the bubbles and the aluminum alloy liquid, and enable the bubbles to capture and absorb more hydrogen and inclusions, thereby improving the dehydrogenation and deslagging effect of gas injection refining. Adding 3-5% by volume of carbon monoxide to the mixed gas is to allow carbon monoxide to capture oxygen in the aluminum alloy liquid to form carbon dioxide, prevent oxygen from forming an aluminum oxide film on the surface of the bubble again with aluminum, enhance the ability of the bubbles to capture and absorb hydrogen and inclusions, and improve the deslagging and dehydrogenation effect of gas injection refining. Through mixed gas injection refining, the hydrogen content of the aluminum alloy liquid can usually be reduced to below 0.15ml / 100gAl, and the inclusion content can be reduced to 0.1mm 2 / kgAl or less, thereby greatly improving the cleanliness of the aluminum alloy liquid.
[0048] Preferably, the mold preheating temperature during extrusion casting in step five is 300-330°C, the pouring temperature of the aluminum alloy liquid is 740-760°C, the extrusion pressure ratio is 150-170MPa, the filling speed is 220-230 mm / s, and the holding time is 18-20 seconds.
[0049] In order to obtain a complete and dense aluminum alloy automobile steering knuckle, the extrusion process parameters must be set reasonably. Since the casting fluidity of the deformed aluminum alloy is worse than that of the aluminum silicon alloy, the extrusion casting molding process of the deformed aluminum alloy automobile steering knuckle cannot refer to the process of the aluminum silicon alloy extrusion casting molding, and the design must be re-optimized. The inventor has conducted a large number of experimental studies on the extrusion casting molding process of the deformed aluminum alloy automobile steering knuckle. The results show that the preheating temperature of the extrusion casting mold must be greater than 300°C, otherwise it is easy to cause incomplete filling of the aluminum alloy automobile steering knuckle or cold shut defects on the surface. The preheating temperature of the mold cannot be too high, otherwise it will increase the cooling time and reduce production efficiency. Preferably, the preheating temperature of the extrusion casting mold is 300-330°C. In addition, the pouring temperature of the aluminum alloy liquid cannot be lower than 740°C, the extrusion pressure cannot be lower than 150MPa, and the filling speed cannot be lower than 220 mm / s, otherwise it will also cause incomplete filling of the aluminum alloy automobile steering knuckle or surface cold shut defects. The pouring temperature of aluminum alloy liquid should not be too high, otherwise it will cause slow cooling and solidification, reducing production efficiency. The extrusion pressure should not be higher than 170MPa, and the filling speed should not be higher than 230mm / s, otherwise it will cause aluminum alloy liquid to splash and entrain in the mold cavity, resulting in pores and loose defects inside the aluminum alloy automobile steering knuckle.
[0050] Preferably, the solution treatment in step seven is to heat and keep the aluminum alloy automobile steering knuckle at 540-550°C for 40-60 minutes, and then put the aluminum alloy automobile steering knuckle into room temperature water and cool it to room temperature, and the aging treatment is to heat and keep the aluminum alloy automobile steering knuckle at 180-190°C for 90-120 minutes, and then cool it to room temperature with the furnace.
[0051] Solution and aging are important means to improve the mechanical properties of aluminum alloy automobile steering knuckles. The solution temperature of existing aluminum alloy automobile steering knuckles is usually 520-530℃. Due to the low solution temperature, it is not only difficult to obtain a supersaturated solid solution, but also leads to a long solution time, which greatly reduces the production efficiency. Similarly, the aging temperature of existing aluminum alloy automobile steering knuckles is usually 150-160℃. Due to the low aging temperature, the aging time is long, which also seriously reduces the production efficiency. Through a large number of experimental explorations and studies, the inventor found that by increasing the solution temperature of the aluminum alloy automobile steering knuckle to 540-550℃, a supersaturated solid solution can be obtained by heating and heat preservation for 40-60 minutes. Similarly, by increasing the aging temperature of the aluminum alloy automobile steering knuckle to 180-190℃, it only takes 90-120 minutes of heating and heat preservation to obtain a high-strength and high-plastic aluminum alloy automobile steering knuckle. At the same time, it can also greatly shorten the heating and heat preservation time, reduce production costs, and improve production efficiency.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] The present invention adopts a deformed aluminum alloy to replace a conventional cast aluminum silicon alloy to extrusion cast an aluminum alloy automobile steering knuckle. By combining powder spray refining and mixed gas refining, the gas slag content of the aluminum alloy liquid is greatly reduced, the damage of pores and inclusions to the mechanical properties of the aluminum alloy automobile steering knuckle is eliminated, and the strength, hardness and plasticity of the aluminum alloy automobile steering knuckle are greatly improved. The tensile strength of the aluminum alloy automobile steering knuckle is greater than 350MPa, the yield strength is greater than 310MPa, the elongation after fracture is greater than 13%, and the Brinell hardness is greater than 105. Compared with the existing extrusion cast aluminum alloy automobile steering knuckle, the strength and hardness of the aluminum alloy automobile steering knuckle of the present invention are improved by more than 5%, and the plasticity is improved by more than 15%. In addition, the aluminum alloy material of the present invention does not contain a large amount of expensive Cu elements, and the heating and heat preservation time of solid solution and aging is shortened, which is conducive to reducing the production cost of the aluminum alloy automobile steering knuckle and promoting the application of the aluminum alloy automobile steering knuckle. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 The microstructure of the aluminum alloy automobile steering knuckle obtained in Example 1 of the present invention.
[0055] Figure 2 The microstructure of the aluminum alloy automobile steering knuckle obtained in Example 2 of the present invention.
[0056] Figure 3 The microstructure of the aluminum alloy automobile steering knuckle obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] Embodiment 1:
[0059] The aluminum alloy automobile steering knuckle is composed of the following components in mass percentage: Mg 1.0%, Si 0.76%, Cu 0.24%, Cr 0.20%, Mn 0.13%, Ti 0.018%, Fe 0.14%, the balance is Al and other inevitable impurities, the content of other impurities is ≤0.05% individually, and the total content of other impurities is ≤0.15%; the extrusion casting production method of the aluminum alloy automobile steering knuckle comprises the following steps in sequence:
[0060] Step 1: Smelting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy automobile steering knuckle;
[0061] Step 2: Use argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.15% of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 710°C for 18 minutes to remove slag and hydrogen, scrape off the scum on the surface of the aluminum alloy liquid, and then let the aluminum alloy liquid stand for 35 minutes;
[0062] Step 3: adding 0.36% of the weight of the aluminum alloy liquid Al-5Ti-1B alloy rod refiner to refine and modify the aluminum alloy liquid;
[0063] Step 4: Use a mixed gas composed of argon, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 710°C for 12 minutes to remove hydrogen and slag. After scraping off the scum on the surface of the aluminum alloy liquid, the aluminum alloy liquid is allowed to stand for 25 minutes. The purity of the argon, sulfur hexafluoride and carbon monoxide is 99.99%. The amount of the mixed gas is 2.5 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.4×10 5 Pa, the volume percentage of sulfur hexafluoride in the mixed gas is 10%, and the volume percentage of carbon monoxide is 4%;
[0064] Step 5: Under the conditions of mold preheating temperature of 315°C, pouring temperature of aluminum alloy liquid of 750°C, extrusion pressure of 160MPa, filling speed of 225mm / s, and holding time of 19 seconds, the aluminum alloy liquid is extruded and cast into an aluminum alloy automobile steering knuckle blank;
[0065] Step 6: Cut off the flash and gate of the aluminum alloy automobile steering knuckle blank;
[0066] Step 7: Heat the aluminum alloy automobile steering knuckle at 545°C for 50 minutes for solution treatment, and then heat the aluminum alloy automobile steering knuckle at 185°C for 100 minutes for aging treatment;
[0067] Step eight: performing surface sandblasting treatment on the aluminum alloy automobile steering knuckle to obtain the aluminum alloy automobile steering knuckle.
[0068] Embodiment 2:
[0069] The aluminum alloy automobile steering knuckle is composed of the following components in mass percentage: Mg 0.98%, Si 0.78%, Cu 0.21%, Cr 0.22%, Mn 0.1%, Ti 0.02%, Fe 0.12%, the balance is Al and other inevitable impurities, the content of other impurities is ≤0.05% individually, and the total content of other impurities is ≤0.15%; the extrusion casting production method of the aluminum alloy automobile steering knuckle comprises the following steps in sequence:
[0070] Step 1: Smelting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy automobile steering knuckle;
[0071] Step 2: Use argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.2% of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 700°C for 20 minutes to remove slag and hydrogen, scrape off the scum on the surface of the aluminum alloy liquid, and then let the aluminum alloy liquid stand for 30 minutes;
[0072] Step 3: adding 0.4% of the weight of the aluminum alloy liquid Al-5Ti-1B alloy rod refiner to refine and modify the aluminum alloy liquid;
[0073] Step 4: Use a mixed gas composed of argon, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 700°C for 10 minutes to remove hydrogen and slag. After scraping off the scum on the surface of the aluminum alloy liquid, the aluminum alloy liquid is allowed to stand for 30 minutes. The purity of the argon, sulfur hexafluoride and carbon monoxide is 99.99%. The amount of the mixed gas is 3 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.3×10 5 Pa, the volume percentage of sulfur hexafluoride in the mixed gas is 9%, and the volume percentage of carbon monoxide is 5%;
[0074] Step 5: Under the conditions of mold preheating temperature of 330°C, pouring temperature of aluminum alloy liquid of 740°C, extrusion pressure of 170MPa, filling speed of 220mm / s, and holding time of 20 seconds, the aluminum alloy liquid is extruded and cast into an aluminum alloy automobile steering knuckle blank;
[0075] Step 6: Cut off the flash and gate of the aluminum alloy automobile steering knuckle blank;
[0076] Step 7: Heat the aluminum alloy automobile steering knuckle at 550°C for 40 minutes for solution treatment, and then heat the aluminum alloy automobile steering knuckle at 180°C for 120 minutes for aging treatment;
[0077] Step eight: performing surface sandblasting treatment on the aluminum alloy automobile steering knuckle to obtain the aluminum alloy automobile steering knuckle.
[0078] Embodiment 3:
[0079] The aluminum alloy automobile steering knuckle is composed of the following components in mass percentage: Mg 1.02%, Si 0.73%, Cu 0.26%, Cr 0.18%, Mn 0.15%, Ti 0.015%, Fe 0.15, and the balance is Al and other inevitable impurities, the content of each impurity is ≤0.05%, and the total content of other impurities is ≤0.15%. The extrusion casting production method of the aluminum alloy automobile steering knuckle comprises the following steps in sequence:
[0080] Step 1: Smelting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy automobile steering knuckle;
[0081] Step 2: Use argon gas with a purity of 99.99% and a powder refining agent with a weight of 0.1% of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 720°C for 15 minutes to remove slag and hydrogen, scrape off the scum on the surface of the aluminum alloy liquid, and then let the aluminum alloy liquid stand for 40 minutes;
[0082] Step 3: adding 0.3% of the weight of the aluminum alloy liquid Al-5Ti-0.2C alloy rod refiner to refine and modify the aluminum alloy liquid;
[0083] Step 4: Use a mixed gas composed of argon, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 720°C for 15 minutes to remove hydrogen and slag. After scraping off the scum on the surface of the aluminum alloy liquid, the aluminum alloy liquid is allowed to stand for 20 minutes. The purity of the argon, sulfur hexafluoride and carbon monoxide is 99.99%. The amount of the mixed gas is 2 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.5×10 5 Pa, the volume percentage of sulfur hexafluoride in the mixed gas is 11%, and the volume percentage of carbon monoxide is 3%;
[0084] Step 5: Under the conditions of mold preheating temperature of 300°C, pouring temperature of aluminum alloy liquid of 760°C, extrusion pressure of 150MPa, filling speed of 230mm / s, and holding time of 18 seconds, the aluminum alloy liquid is extruded and cast into an aluminum alloy automobile steering knuckle blank;
[0085] Step 6: Cut off the flash and gate of the aluminum alloy automobile steering knuckle blank;
[0086] Step 7: Heat the aluminum alloy automobile steering knuckle at 540°C for 60 minutes for solution treatment, and then heat the aluminum alloy automobile steering knuckle at 1190°C for 90 minutes for aging treatment;
[0087] Step eight: performing surface sandblasting treatment on the aluminum alloy automobile steering knuckle to obtain the aluminum alloy automobile steering knuckle.
[0088] The powder refining agent in step 1 of Example 1-3 of the present invention is composed of the following components in percentage by mass: NaCl 35.12%, NaF 19.84%, TiCl 3 16.51%, SrSO 4 10.06%, KPO 3 11.45%, Na 2 B 4 O 7 7.02%, the preparation method of the powder refining agent comprises the following steps in sequence: (1) according to the composition and mass percentage of the powder refining agent, NaCl, NaF, TiCl with a purity of 99.8% are selected; 3 、SrSO 4 , KPO3 、Na 2 B 4 O 7 The steps of: (1) preparing ingredients for the raw materials; (2) adding the ingredients into water at a temperature of 70° C. and stirring to dissolve the ingredients into an aqueous solution, wherein the mass ratio of water to the ingredients is 1.2, and then heating the aqueous solution to 100° C. to evaporate the aqueous solution to obtain solid crystals; and (3) crushing the solid crystals into powders with a particle size of less than 2 mm, and drying and dehydrating the powders at 160° C. for 4 hours to obtain the powder refining agent.
[0089] Comparative Example 1:
[0090] The composition, mass percentage and extrusion casting production method of the aluminum alloy automobile steering knuckle of this comparative example are the same as those of Example 1, except that the powder refining agent used is a conventional powder refining agent available on the market, and the powder refining agent is composed of the following components in mass percentage: NaCl 36.13%, KCl 15.42%, CaF 2 16.84%, NaF 19.24%, C 2 Cl 6 12.37%, the powder refining agent is obtained by directly crushing and mixing the raw materials after drying and dehydration.
[0091] Comparative Example 2:
[0092] The component composition, mass percentage and extrusion casting production method of the aluminum alloy automobile steering knuckle in this comparative example are the same as those in Example 1, except that in step three, no mixed gas is used to spray, refine, remove hydrogen and remove slag on the aluminum alloy liquid, but argon gas with a purity of 99.99% is used to spray, refine, remove hydrogen and remove slag on the aluminum alloy liquid.
[0093] Verification example:
[0094] The hydrogen content and slag content of the aluminum alloy liquid before extrusion casting of Examples 1-3 and Comparative Examples 1-2 were tested on site using a HDA-V hydrogen meter and an Analyze PoDFA slag meter. The results are shown in Table 1. As can be seen from Table 1, the hydrogen content of the aluminum alloy liquid of Examples 1-3 is less than 0.15 ml / 100 gAl, and the slag content is less than 0.1 mm 2 / kgAl. Comparative Example 1 uses a commercially available conventional powder refining agent for spray refining, and Comparative Example 2 does not use a mixed gas for spray refining, resulting in a relatively high gas slag content in the aluminum alloy liquid. By comparison, it can be seen that the technical solution of the present invention can significantly reduce the gas slag content of the aluminum alloy liquid before squeeze casting and improve the cleanliness of the squeeze cast aluminum alloy automobile steering knuckle.
[0095] Table 1 Hydrogen content and slag content of aluminum alloy liquid
[0096]
[0097]
[0098] Samples were taken from the aluminum alloy automobile steering knuckles obtained in Examples 1-3. After grinding, polishing and corrosion, the microstructure of the samples was observed under an optical microscope. Figure 1-3 The microstructures of the aluminum alloy automobile steering knuckles obtained in Examples 1-3 are respectively shown. Samples were taken from the aluminum alloy automobile steering knuckles obtained in Examples 1-3 and Comparative Examples 1-2 to test the tensile mechanical properties and Brinell hardness of the aluminum alloy automobile steering knuckles, and the results are shown in Table 2. As can be seen from Table 2, the tensile strength of the aluminum alloy automobile steering knuckles in Examples 1-3 is greater than 350MPa, the yield strength is greater than 310MPa, the elongation after fracture is greater than 13%, and the Brinell hardness is greater than 105. While the tensile strength of the aluminum alloy automobile steering knuckles in Comparative Examples 1 and 2 is lower than 330MPa, the yield strength is lower than 300MPa, the elongation after fracture is lower than 12%, and the Brinell hardness is lower than 100. By comparison, it can be seen that the strength and hardness of the aluminum alloy automobile steering knuckles in Examples 1-3 are improved by more than 5%, and the plasticity is improved by more than 15%.
[0099] Table 2 Tensile mechanical properties and Brinell hardness of aluminum alloy automobile steering knuckle
[0100]
Claims
1. An aluminum alloy automobile steering knuckle, characterized in that: The aluminum alloy automobile steering knuckle is composed of the following components in mass percentage: Mg 0.98-1.02%, Si 0.73-0.78%, Cu 0.21-0.26%, Cr 0.18-0.22%, Mn 0.1-0.15%, Ti 0.015-0.02%, Fe≤0.15%, and the balance is Al and other inevitable impurities, the content of each other impurity is ≤0.05%, and the total content of other impurities is ≤0.15%.
2. A method for producing an aluminum alloy automobile steering knuckle by extrusion casting as claimed in claim 1, characterized in that: The following steps are included in sequence: Step 1: Smelting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy automobile steering knuckle; Step 2: using inert gas and powder refining agent to spray and refine the aluminum alloy liquid to remove slag and hydrogen; Step 3: Adding a refiner to refine and modify the aluminum alloy liquid; Step 4: using mixed gas to spray and refine the aluminum alloy liquid to remove hydrogen and slag; Step 5: Extrusion casting the aluminum alloy liquid into an aluminum alloy automobile steering knuckle blank; Step 6: Cut off the flash and gate of the aluminum alloy automobile steering knuckle blank; Step 7: Perform solid solution and aging treatment on the aluminum alloy automobile steering knuckle; Step eight: performing surface sandblasting treatment on the aluminum alloy automobile steering knuckle to obtain the aluminum alloy automobile steering knuckle.
3. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2 is characterized in that: The inert gas in step 2 is argon with a purity of ≥99.99%, the amount of the powder refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during the spray refining is 700-720°C, and the spray refining time is 15-20 minutes.
4. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2 is characterized in that: The powder refining agent in step 2 is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method of the powder refining agent comprises the following steps in sequence: (1) according to the composition and mass percentage of the powder refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70°C and stirred to dissolve into an aqueous solution, the mass ratio of water to ingredients being 1.2, and then the aqueous solution is heated to 100°C to evaporate to obtain solid crystals; (3) the solid crystals are crushed into powders with a particle size of less than 2 mm, and the powders are dried and dehydrated at 160°C for 4 hours to obtain the powder refining agent.
5. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2 is characterized in that: The refiner in step 3 is an Al-5Ti-1B alloy rod or an Al-5Ti-0.2C alloy rod, and the amount of the refiner added is 0.3-0.4% of the weight of the aluminum alloy liquid.
6. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2, characterized in that: The mixed gas in step 4 is composed of argon gas with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide, the volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, and the volume percentage of carbon monoxide is 3-5%.
7. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2, characterized in that: The amount of the mixed gas in step 4 is 2-3 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is (0.3-0.5)×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.
8. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2, characterized in that: In step 5, the preheating temperature of the extrusion casting mold is 300-330° C., the pouring temperature of the aluminum alloy liquid is 740-760° C., the extrusion pressure ratio is 150-170 MPa, the filling speed is 220-230 mm / s, and the holding time is 18-20 seconds.
9. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2, characterized in that: The solid solution treatment in step seven is to heat the aluminum alloy automobile steering knuckle at 540-550° C. for 40-60 minutes, and then put the aluminum alloy automobile steering knuckle into room temperature water and cool it to room temperature.
10. The extrusion casting production method of aluminum alloy automobile steering knuckle according to claim 2, characterized in that: The aging process described in step seven is to heat the aluminum alloy automobile steering knuckle at 180-190° C. for 90-120 minutes and then cool it to room temperature along with the furnace.