Nodular cast iron material, composition containing nodular cast iron material, brake head and preparation method of nodular cast iron material

By controlling the composition and processing technology of ductile iron materials, high-strength and high-plasticity ductile iron was produced, solving the problem that existing materials could not meet the requirements of brake shoe torsion, and achieving the improvement of material performance and the reduction of manufacturing costs.

CN119040734APending Publication Date: 2024-11-29CRRC QIQIHAR ROLLING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411157290.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing ductile iron materials cannot meet the requirements for high-quality brake shoe tors, especially due to insufficient elongation, which prevents them from simultaneously possessing high strength and good toughness.

Method used

By controlling the composition ratio of ductile iron materials, including the content of C, Si, Cu, Mn, P, and S, and combining the use of spheroidizing agents and inoculants, spheroidizing and inoculating treatments are carried out to prepare ductile iron materials with a mixed ferrite and pearlite structure.

Benefits of technology

A ductile iron material with high yield strength, tensile strength and elongation of over 18% was obtained, which has high strength and good plasticity, meets the requirements of high-quality brake shoe tors, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040734A_ABST
    Figure CN119040734A_ABST
Patent Text Reader

Abstract

The invention provides a nodular cast iron material, a composition containing the nodular cast iron material, a brake head and a preparation method of the nodular cast iron material, and the nodular cast iron material comprises the following components in percentage by mass: 3.35%-3.81% of C, 2.35%-2.75% of Si, 0.1%-0.28% of Cu, 0.15%-0.33% of Mn, less than or equal to 0.03% of P, less than or equal to 0.02% of S and the balance of iron and inevitable impurities. Nodular cast iron manufactured based on the nodular cast iron material not only has high strength, but also has good plasticity, and can meet the requirement for manufacturing a high-quality brake head.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy materials, and in particular to a ductile iron material, a composition containing the same, a brake shoe support and a preparation method of the ductile iron material. Background Art

[0002] The braking form of railway freight cars generally adopts single-sided brake shoe braking. The braking device mainly includes brake beams, levers, brake shoe supports and other components. Since the brake shoe supports are subjected to greater stress during the braking process, the material of the brake shoe supports is required to have not only high strength but also good toughness, so high quality requirements are required for it.

[0003] At present, the material of brake shoe support is cast steel. Ductile iron refers to cast iron in which graphite is distributed in the iron matrix in a spherical shape in the microstructure. It is a high-strength cast iron material developed in the 1950s. Its comprehensive performance is close to that of steel, and it has excellent casting performance. It has been successfully used to cast some parts with complex forces and high requirements for strength, toughness and wear resistance. The mechanical properties of ductile iron in my country's national standard GB / T1348 "Ductile Iron Parts" are shown in Table 1. The elongation of ductile iron in Table 1 is too low and cannot meet the market's requirements for high-quality brake shoe support.

[0004] Table 1. Mechanical properties of ductile iron in national standard GB / T1348

[0005] Material grade Tensile strength Rm / MPa(min) Yield strength Rp0.2 / MPa(min) Elongation A / %(min) QT450-10 450 310 10 QT500-7 500 320 7 QT550-5 550 350 5 QT600-3 600 370 3 QT700-2 700 420 2 QT800-2 800 480 2 QT900-2 900 600 2 Summary of the invention

[0006] The main purpose of the present invention is to provide a ductile iron material, a composition containing the same, a brake shoe holder and a preparation method of the ductile iron material, so as to solve the problem that the ductile iron material in the prior art cannot meet the requirements for preparing high-quality brake shoe holders.

[0007] In order to achieve the above-mentioned object, according to one aspect of the present invention, a ductile iron material is provided, which comprises the following components, in terms of mass percentage: C 3.35% to 3.81%, Si 2.35% to 2.75%, Cu 0.1% to 0.28%, Mn 0.15% to 0.33%, P≤0.03%, S≤0.02%, and the balance is iron and unavoidable impurities.

[0008] Furthermore, the ductile iron material comprises the following components in percentage by mass: C 3.55% to 3.80%, Si 2.55% to 2.70%, Cu 0.18% to 0.28%, Mn 0.20% to 0.33%, P≤0.03%, S≤0.02%, and the remainder is iron and unavoidable impurities.

[0009] According to another aspect of the present invention, a ductile iron composition is provided, comprising a ductile iron material, a spheroidizer and an inoculant, wherein the ductile iron material is the ductile iron material as described above.

[0010] Furthermore, the weight ratio of the spheroidizing agent, the inoculant and the ductile iron material is 1-2:0.5-1.5:100.

[0011] Furthermore, the inoculant comprises the following components by weight percentage: C≤0.20%, Si 72.0%-80.0%, Mn≤0.50%, P≤0.030%, S≤0.020%, Cr≤0.50%, Al 0.1%-0.5%, and the balance is iron and unavoidable impurities.

[0012] Furthermore, the spheroidizer is a rare earth magnesium spheroidizer, and the rare earth magnesium spheroidizer comprises the following components by weight percentage: C < 0.1%, 2.58% < RE ≤ 4.5%, 4% < Mg ≤ 5.3%, 30% < Si ≤ 40.0%, Ca 2.0% to 4.0%, 0.8% < Al < 1.0%, Ti < 0.5%, and the balance is iron and unavoidable impurities.

[0013] According to another aspect of the present invention, a method for preparing ductile iron is provided, which is prepared from the above ductile iron composition, and the preparation steps are as follows:

[0014] Step S1, smelting ductile iron material to obtain molten iron;

[0015] Step S2, spheroidizing and inoculating the molten iron under the action of a spheroidizing agent and an inoculant;

[0016] Step S3, casting the spheroidized and inoculated molten iron to obtain ductile iron.

[0017] Furthermore, the smelting furnace temperature is 1450°C to 1500°C.

[0018] Further, the spheroidization and inoculation steps are as follows:

[0019] The molten iron is subjected to bottom spheroidization and the first inoculation by using a spheroidizer and a part of an inoculant; the content of the part of an inoculant is 1.0% to 1.4% by weight of the ductile iron composition; after the bottom spheroidization and the first inoculation are completed, slag removal is performed, and after the slag removal is completed, the remaining inoculant is added for the second inoculation.

[0020] Furthermore, the casting temperature is 1350°C to 1400°C.

[0021] Furthermore, step S3 also includes performing a sand dropping operation after the casting is completed. The conditions for the sand dropping operation are to control the sand dropping time to 2.5h to 3h at an ambient temperature below 5°C or to control the sand dropping time to 1.5h to 2h at an ambient temperature above 5°C.

[0022] According to another aspect of the present invention, a brake shoe holder is provided. The material of the brake shoe holder is ductile iron prepared by the above method for preparing ductile iron.

[0023] Furthermore, the brake shoe support comprises a brake shoe support body, a sliding block and a mounting seat, the mounting seat is arranged between the outer side of the brake shoe support body and the sliding block, and the mounting seat is respectively welded to the outer side of the brake shoe support body and the sliding block.

[0024] By applying the technical scheme of the present invention, ductile iron with high yield strength, tensile strength and elongation (elongation reaches more than 18%) is obtained by controlling the composition of ductile iron materials and the content of each component. The ductile iron made of ductile iron materials with the above composition not only has high strength, but also has good plasticity, which can meet the requirements of manufacturing high-quality brake shoe supports; and compared with cast steel, ductile iron has excellent casting properties. Using ductile iron as the preparation material of the brake shoe support can improve the casting processability of the brake shoe support and reduce the manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0026] Figure 1 It shows a schematic structural diagram of a brake shoe support according to an embodiment of the present invention;

[0027] Figure 2 It shows a schematic diagram of the structure of the brake shoe support after being decomposed according to an embodiment of the present invention;

[0028] Figure 3 The metallographic structure diagram of ductile iron prepared according to Example 19 of the present invention is shown.

[0029] The above drawings include the following reference numerals:

[0030] 1. Watt support body; 3. Slider; 2. Mounting seat. DETAILED DESCRIPTION

[0031] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0032] As described in the background technology, the ductile iron material existing in the prior art cannot meet the requirements for preparing high-quality brake shoe support. In order to solve the above problem, according to one aspect of the present invention, a ductile iron material is provided, which comprises the following components in mass percentage: C 3.35% to 3.81%, Si 2.35% to 2.75%, Cu 0.1% to 0.28%, Mn 0.15% to 0.33%, P≤0.03%, S≤0.02%, and the balance is iron and unavoidable impurities.

[0033] In the ductile iron preparation process, by controlling the content of each chemical element of the ductile iron material within a reasonable range and utilizing the synergistic effect of each element, the matrix structure of the prepared ductile iron is a mixed structure of ferrite and pearlite, with a lower pearlite content, a higher ferrite content and almost no intergranular carbide, so that the plasticity of ferrite is fully exerted, the generation and expansion of cracks are suppressed, and the ductile iron material is ensured to have higher strength and better plasticity. Specifically, the inventors of the present application have found that the carbon and silicon content affects the amount, size, roundness and matrix strength of the precipitated graphite. In order to ensure the carbon equivalent, graphitization effect (a large number of graphite balls, a small ball diameter, and a high roundness), fewer intergranular carbides and give full play to the solid solution strengthening effect of silicon, the carbon content is controlled at 3.35% to 3.81% and the Si content is controlled at 2.35% to 2.75%; the copper element promotes the formation of a small amount of pearlite and refines the pearlite lamella spacing on the basis of giving full play to the solid solution strengthening effect. The copper content is controlled at 0.1% to 0.28%, which is conducive to the formation of less pearlite and intergranular carbides to ensure the strength and plasticity of the material; the manganese content is controlled at 0.15% to 0.34% and the phosphorus content is controlled at ≤0.03%, which is conducive to avoiding component segregation and intergranular carbide formation, avoiding the generation of brittle phases and ensuring the tensile strength and yield strength of the material. The present invention obtains a ductile iron material with high yield strength, tensile strength and elongation (elongation reaches more than 18%) by controlling the composition of the ductile iron material and the content of each component. The ductile iron made of the ductile iron material with the above composition not only has high strength but also has good plasticity, which can meet the requirements of manufacturing high-quality brake shoe supports. Compared with cast steel, ductile iron has excellent casting properties. Using ductile iron as the preparation material of the brake shoe support can improve the casting processability of the brake shoe support and reduce the manufacturing cost.

[0034] In order to further improve the strength and plasticity of ductile iron, in a preferred embodiment, the ductile iron material contains the following components in mass percentage: C 3.55%-3.80%, Si 2.55%-2.70%, Cu 0.18%-0.28%, Mn 0.20%-0.33%, P≤0.03%, S≤0.02%, and the balance is iron and unavoidable impurities.

[0035] According to another aspect of the present invention, a ductile iron composition is provided, comprising a ductile iron material, a spheroidizing agent and an inoculant, wherein the ductile iron material is the ductile iron material as described above. The composition comprising the ductile iron material can be used to prepare ductile iron with excellent mechanical properties, which can meet the requirements of manufacturing high-quality brake shoe support.

[0036] In a preferred embodiment, the weight ratio of the spheroidizing agent, the inoculant and the ductile iron material is 1-2: 0.5-1.5: 100. The main function of the inoculant is to promote graphitization, improve the graphite morphology and distribution, and refine the matrix structure. The main function of the spheroidizing agent is to promote the formation of spheroidal graphite. The above dosage ratio can obtain ductile iron with good mechanical properties.

[0037] In a preferred embodiment, the inoculant comprises the following components by weight percentage: C≤0.20%, Si72.0-80.0%, Mn≤0.50%, P≤0.030%, S≤0.020%, Cr≤0.50%, Al 0.1%-0.5%, and the balance is iron and unavoidable impurities.

[0038] In a preferred embodiment, the spheroidizing agent is a rare earth magnesium spheroidizing agent, and the rare earth magnesium spheroidizing agent contains the following components by weight percentage: C < 0.1%, 2.58% < RE ≤ 4.5%, 4% < Mg ≤ 5.3%, 30% < Si ≤ 40.0%, Ca 2.0% ~ 4.0%, 0.8% < Al < 1.0%, Ti < 0.5%, and the balance is iron and inevitable impurities. The spheroidizing agent adopts a lower magnesium content and a higher RE content, so that the spheroidizing reaction is relatively gentle, the spheroidizing element absorption rate is high, the anti-decay performance is good, and a good and stable spheroidizing effect is guaranteed; the use of a lower silicon content can avoid excessive silicon addition of the spheroidizing agent, which is conducive to controlling the silicon content in the original iron water to ensure a good spheroidizing effect, inoculation effect and ferrite content. Calcium is a desulfurization element. Controlling its content within the above range can effectively desulfurize to reduce the consumption of RE and magnesium and improve the spheroidizing effect.

[0039] According to another aspect of the present invention, a method for preparing ductile iron is provided, which is prepared from the above ductile iron composition, and the preparation steps are as follows: step S1, smelting the ductile iron material to obtain molten iron; step S2, spheroidizing and inoculating the molten iron under the action of a spheroidizing agent and an inoculant; step S3, casting the spheroidized and inoculated molten iron to obtain ductile iron. By controlling the content of each chemical element of the ductile iron material within a reasonable range, and ensuring the roundness of graphite and the size of graphite balls, and the relative content of pearlite and ferrite in the matrix structure through subsequent spheroidizing and inoculating treatment, finally, graphite with good spheroidization and appropriate relative content of pearlite and ferrite is obtained, so as to achieve simultaneous improvement of the strength and plasticity of the ductile iron, thereby obtaining ductile iron with both high strength and high plasticity, which can meet the requirements for preparing high-quality brake shoe support.

[0040] In order to further improve the mechanical properties of ductile iron, in a preferred embodiment, the smelting furnace temperature is 1450°C to 1500°C.

[0041] In a preferred embodiment, the spheroidizing and inoculating steps are as follows: the molten iron is subjected to bottom spheroidizing and the first inoculation with a spheroidizing agent and a part of the inoculant; the content of the part of the inoculant is 1.0% to 1.4% by weight of the ductile iron composition; after the bottom spheroidizing and the first inoculation are completed, slag is removed, and after the slag removal is completed, the remaining inoculant is added for a second inoculation, and the molten iron after the second inoculation is subsequently cast to obtain ductile iron.

[0042] In order to further improve the mechanical properties of ductile iron, in a preferred embodiment, the casting temperature is 1350° C. to 1400° C. Controlling the casting temperature within the above range can, on the one hand, avoid the defects of slow solidification and easy growth of grain structure due to too high casting temperature, and on the other hand, avoid the defects of difficult filling of molten iron, poor density of castings, easy formation of shrinkage cavities, shrinkage and porosity due to too low casting temperature.

[0043] In order to ensure that the ductile iron obtained after casting has a better surface structure, in a preferred embodiment, step S3 also includes a sand dropping operation after the casting is completed, and the sand dropping operation conditions are to control the sand dropping time to 2.5h~3h at an ambient temperature below 5°C or to control the sand dropping time to 1.5h~2h at an ambient temperature greater than 5°C.

[0044] According to yet another aspect of the present invention, a brake shoe support is provided. The material of the brake shoe support is ductile iron prepared by the above method for preparing ductile iron.

[0045] like Figure 1As shown, in a preferred embodiment, the brake shoe support includes a brake shoe support body 1, a slider 3 and a mounting seat 2, the mounting seat 2 is arranged between the outer side of the brake shoe support body 1 and the slider 3, and the mounting seat 2 is welded to the outer side of the brake shoe support body 1 and the slider 3 respectively.

[0046] In the prior art, the slider and the main body of the brake shoe support are cast together in an integrated structure. Since two different brake shoe supports are installed on the same brake beam, two different molds are required. In addition, due to the different angles and positions of the sliders, the brake shoe supports with sliders cannot be used interchangeably, resulting in a large number of brake shoe types and brake shoe molds, high manufacturing costs and difficulty in management. The present invention adopts a split structure, such as Figure 2 As shown, ductile iron is used to prepare the brake shoe support body, the slider and the mounting seat respectively, and then the three are fixed together by welding, thereby reducing the number of brake shoe support casting molds and reducing manufacturing costs.

[0047] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0048] Examples 1 to 18

[0049] The composition and content (mass percentage content) of the ductile iron materials of Examples 1 to 20 are shown in Table 2, respectively, and the remainder is iron and unavoidable impurities.

[0050] Embodiment 19

[0051] The ductile iron material of Example 1 was used to prepare ductile iron. The specific parameters are shown in Table 3. The specific steps are as follows:

[0052] 1) 500 kg of ductile iron material is placed in a smelting process to obtain molten iron, and the smelting outlet temperature is controlled to be 1480°C.

[0053] 2) Using ladle bottom spheroidization, 8kg spheroidizer and 6kg inoculant are placed in the ladle in sequence, and then covered with a layer of 1kg K-34# slag collector (Qingdao Fusai Ke Casting Materials Co., Ltd.), and molten iron is poured into the ladle for spheroidization and the first inoculation.

[0054] 3) After the spheroidization treatment and the first inoculation are completed, the slag is removed. After the slag removal, 1 kg of inoculant is added for the second inoculation to obtain the inoculated molten iron.

[0055] 3) After the second inoculation, the temperature of the molten iron is cooled to 1400° C. before casting; wherein, coated sand is used to prepare a Y-type test block casting mold, and the floating sand in the sand mold is purged before casting.

[0056] 4) The sand dropping time is controlled to be 1.5 hours at 15°C to obtain ductile iron in a Y-type test block mold.

[0057] Among them, the element composition and content (mass percentage content) of the spheroidizer used are shown in Table 4, and the balance is and inevitable impurities; the element composition and content (mass percentage content) of the inoculant used are shown in Table 5, and the balance is iron and inevitable impurities.

[0058] Examples 20 to 36

[0059] The only difference between it and Example 19 is that the specific parameters in the preparation process of ductile iron, the elemental composition of the spheroidizing agent and the elemental composition of the inoculant are different; specifically, the specific parameters in the preparation process are shown in Table 3; the elemental composition of the spheroidizing agent used is shown in Table 4, and the balance is and inevitable impurities; the elemental composition of the inoculant used is shown in Table 5, and the balance is iron and inevitable impurities.

[0060] Embodiment 37

[0061] The only difference between it and Example 19 is that the composition of the ductile iron material is different. Specifically, the ductile iron material contains the following components by mass percentage: C 3.35%, Si 2.35%, Mn 0.20%, Cu 0.18%, P 0.03%, S 0.02%, and the balance is iron and inevitable impurities.

[0062] Embodiment 38

[0063] The only difference between this embodiment and Example 19 is that the composition of the ductile iron material is different. Specifically, the ductile iron material comprises the following components by mass percentage: C 3.81%, Si 2.75%, Mn 0.33%, Cu 0.28%, P 0.03%, S 0.02%, and the balance is iron and unavoidable impurities.

[0064] Embodiment 39

[0065] The only difference between it and Example 19 is that the spheroidizing agent is different, as shown in Table 4.

[0066] Comparative Example 1

[0067] The only difference from Example 19 is that the manganese content in the ductile iron material is 0.45%.

[0068] Comparative Example 2

[0069] The only difference between it and Example 19 is that the copper content in the ductile iron material is 0.42%.

[0070] Comparative Example 3

[0071] The only difference between it and Example 19 is that the P content in the ductile iron material is 0.035%.

[0072] Table 2. Element composition and content of ductile iron materials

[0073]

[0074]

[0075] Table 3. Specific parameters in the preparation process of ductile iron

[0076]

[0077] Table 4. Element composition and content of spheroidizing agent

[0078]

[0079]

[0080] Table 5. Element composition and content of inoculant

[0081] C(%) Si(%) Mn(%) P(%) S(%) Cr(%) Al(%) Embodiment 19 0.20 72.4 0.45 0.021 0.011 0.18 0.39 Embodiment 20 0.18 72.5 0.41 0.022 0.012 0.20 0.40 Embodiment 21 0.19 72.4 0.44 0.023 0.012 0.21 0.35 Embodiment 22 0.18 72.3 0.43 0.022 0.010 0.19 0.39 Embodiment 23 0.20 72.5 0.44 0.021 0.012 0.20 0.40 Embodiment 24 0.19 72.4 0.43 0.021 0.011 0.20 0.40 Embodiment 25 0.18 72.5 0.43 0.023 0.013 0.21 0.35 Embodiment 26 0.18 72.4 0.44 0.023 0.010 0.21 0.40 Embodiment 27 0.19 72.4 0.42 0.021 0.013 0.19 0.35 Embodiment 28 0.19 80.0 0.43 0.020 0.020 0.20 0.40 Examples 29 to 35 0.19 72.4 0.43 0.021 0.011 0.20 0.37 Embodiment 36 0.20 70.0 0.43 0.021 0.011 0.20 0.37

[0082] Performance Test:

[0083] (1) The microstructure of the ductile iron prepared in Example 19 was tested and the following results were obtained: Figure 3 The metallographic structure shown in Figure 3 It can be seen that the ductile iron of the present invention has a lower pearlite content and a higher ferrite content, and almost no intergranular carbide.

[0084] (2) The tensile strength, yield strength and elongation of the ductile iron prepared in the embodiment and the comparative example were tested using the GB / T 1348-2009 standard. The test results are shown in Table 6. Since the existing ductile iron materials in my country cannot meet the requirements of the new standard for brake shoe supports, some manufacturers have proposed new standards for the ductile iron brake shoe supports they purchased, as shown in Table 6.

[0085] Table 6. Test results of tensile strength, yield strength and elongation of ductile iron

[0086]

[0087]

[0088] It can be seen from the data in Table 6 that the ductile iron prepared using the ductile iron material of the present application has yield strength, tensile strength and elongation (elongation reaches more than 18%) that meet the requirements of the new standard, has high strength, plasticity and toughness, and can be used to prepare brake shoe supports.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A ductile iron material, It is characterized in that Calculated by mass percentage, the present invention comprises the following components: C 3.35% to 3.81%, Si 2.35% to 2.75%, Cu 0.1% to 0.28%, Mn 0.15% to 0.33%, P≤0.03%, S≤0.02%, and the balance is iron and unavoidable impurities.

2. The ductile iron material according to claim 1, It is characterized in that The ductile iron material comprises the following components in percentage by mass: C 3.55%-3.80%, Si 2.55%-2.70%, Cu 0.18%-0.28%, Mn 0.20%-0.33%, P≤0.03%, S≤0.02%, and the remainder is iron and unavoidable impurities.

3. A ductile iron composition comprising a ductile iron material, a spheroidizing agent and an inoculant, It is characterized in that The ductile iron material is the ductile iron material according to claim 1 or 2.

4. The ductile iron composition according to claim 3, It is characterized in that The weight ratio of the spheroidizing agent, the inoculant and the ductile iron material is 1 to 2: 0.5~1.5:100。 5. The ductile iron composition according to claim 3, It is characterized in that The inoculant comprises the following components by weight percentage: C≤0.20%, Si 72.0%-80.0%, Mn≤0.50%, P≤0.030%, S≤0.020%, Cr≤0.50%, Al 0.1%-0.5%, and the balance is iron and unavoidable impurities.

6. The ductile iron composition according to any one of claims 3 to 5, It is characterized in that The spheroidizer is a rare earth magnesium spheroidizer, and the rare earth magnesium spheroidizer comprises the following components by weight percentage: C < 0.1%, 2.58% < RE ≤ 4.5%, 4% < Mg ≤ 5.3%, 30% < Si ≤ 40.0%, Ca 2.0% to 4.0%, 0.8% < Al < 1.0%, Ti < 0.5%, and the balance is iron and unavoidable impurities.

7. A method for preparing ductile iron, It is characterized in that The ductile iron composition is prepared from any one of claims 3 to 6, and the preparation steps are as follows: Step S1, smelting ductile iron material to obtain molten iron; Step S2, spheroidizing and inoculating the molten iron under the action of a spheroidizing agent and an inoculant; Step S3, casting the molten iron after spheroidization and inoculation to obtain the ductile iron.

8. The method for preparing ductile iron according to claim 7, It is characterized in that The smelting furnace temperature is 1450°C to 1500°C; and / or, The spheroidization and inoculation steps are as follows: The molten iron is subjected to bottom spheroidization and first inoculation by using the spheroidizer and part of the inoculant; the content of the part of the inoculant is 1.0% to 1.4% by weight of the ductile iron composition; after the bottom spheroidization and first inoculation are completed, slag is removed, and after the slag removal is completed, the remaining inoculant is added to perform a second inoculation; and / or, the casting temperature is 1350° C. to 1400° C.; and / or, The step S3 also includes performing a sand dropping operation after the casting is completed. The sand dropping operation condition is to control the sand dropping time to 2.5h to 3h at an ambient temperature below 5°C or to control the sand dropping time to 1.5h to 2h at an ambient temperature above 5°C.

9. A brake shoe support, It is characterized in that The material of the brake shoe support is ductile iron prepared by the method for preparing ductile iron according to claim 7 or 8.

10. The brake shoe holder according to claim 9, It is characterized in that The invention comprises a brake shoe support body, a sliding block and a mounting seat, wherein the mounting seat is arranged between the outer side of the brake shoe support body and the sliding block, and the mounting seat is respectively welded to the outer side of the brake shoe support body and the sliding block.

Citation Information

Cited By

  • Nodular cast iron material, composition containing same, brake head and preparation method for nodular cast iron material

    WO2026040709A1