High-strength invar steel wire and peeling-free high-yield preparation method thereof
By adopting specific chemical composition design and process flows in the preparation process of high-strength Inner steel wire materials, including solid solution treatment and surface treatment, the problems of poor surface treatment materials in the prior art are solved, and high The material yield and low cost production are maintained while maintaining the excellent performance of the material.
Patent Information
- Application Number
- CN202411006100.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-29
AI Technical Summary
The surface treatment process of existing high-strength Inner steel wire materials has problems such as large material loss and poor pickling effect, which affects the quality of subsequent aluminum-covered or galvanized processes.
The chemical composition design of high-strength steel wire material and the preparation method without peeling and high material yield is adopted, including vacuum smelting, electroslag refining, forging, strip rolling, solid solution treatment, strip surface treatment, wire cold drawing and heat treatment processes. Through processes such as shot blasting, alkaline washing-pickling-phosphorization-saponification, electrolytic pickling and hydrogen atmosphere online annealing, the oxide scale is removed and the formation of the oxide layer is reduced.
It effectively reduces the formation of oxide scale, improves the surface treatment quality of silk material, reduces material loss, reduces production costs, and maintains the performance of high conductivity and low thermal expansion coefficient.
Smart Images

Figure CN119040739A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of low expansion alloys, and in particular relates to a high-strength invar steel wire and a peeling-free high-yield preparation method thereof. Background Art
[0002] Invar, also known as Invar alloy, is widely used in electrical instruments, energy transportation, communication equipment and other fields due to its low expansion coefficient. In recent years, high-strength Invar wires formed by strengthening traditional Invar through solid solution strengthening, work hardening, aging strengthening and other methods have shown great application potential in the field of power transportation and are irreplaceable key core materials for the preparation of double-capacity conductors.
[0003] The preparation process of high-strength Invar wire mainly includes smelting, forging (or continuous rolling), wire rod rolling, wire rod heat treatment, wire drawing and wire annealing. In the wire rod rolling and wire rod heat treatment processes, the Invar steel will be heated at high temperatures, which can be as high as 1100°C or above, resulting in a thicker oxide scale on the surface of the wire rod, affecting the surface quality of the wire rod. In the field of power transmission lines, Invar wire is usually aluminum-clad or galvanized, so the surface quality requirements of Invar wire are high and it needs to be surface treated.
[0004] At present, the surface treatment methods of Invar wire include peeling and pickling. Peeling usually results in a large material loss (about 10%), resulting in waste of resources and increased costs. Due to the constraints of the production line, the pickling production line and process of high-strength Invar wire are the same as those of carbon steel wire, and the pickling process of hydrochloric acid or sulfuric acid is usually used. However, due to the different corrosion resistance of Invar and carbon steel, the pickling effect is usually poor, which affects the subsequent aluminum or galvanizing process. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a high-strength Invar steel wire and a peeling-free high-yield preparation method thereof, which improves the quality of wire surface treatment and reduces production costs while avoiding material loss caused by wire peeling.
[0006] The technical scheme adopted by the present invention is: a high-strength invar steel wire material, the chemical composition and mass percentage of which are: C: 0.09-0.32%, Ni: 37.0-38.0%, Mo: 0.3-0.5%, Cr: 0.5-0.7%, Co: 0.6-0.9%, Mn: 0.1-0.3%, Ti≤0.01%, Si: 0.1-0.2%, P≤0.02%, S≤0.01%, and the balance is iron and inevitable impurities; wherein the mass percentage of Cr, Mo, Co and Ni elements satisfies the relationship: Co=Cr+0.4Mo±0.05, and Co+Ni≤38.6%.
[0007] Furthermore, the wire has a diameter of 3.0 to 5.5 mm, a tensile strength of ≥1250 MPa, and a thermal expansion coefficient of ≤2.5×10 -6 / ℃, electrical conductivity ≥2%IACS at 20℃.
[0008] The above-mentioned high-strength Invar steel wire material is prepared without peeling and with high yield rate, comprising vacuum melting, electroslag refining, forging, wire rod rolling, solution treatment, wire rod surface treatment, wire cold drawing, and wire heat treatment steps;
[0009] In the solution treatment process, before the wire rod is loaded into the furnace, the heating furnace is preheated, the temperature is raised to 800-850°C and then the wire rod is loaded into the furnace; then the temperature is raised to 1130-1150°C and the temperature is kept at t1=1.8+0.15D1; then the wire rod is taken out of the furnace and water-cooled; t1 is the holding time, h; D1 is the diameter of the wire rod after rolling, mm;
[0010] In the wire rod surface treatment process, the wire rod is shot blasted, and then alkali-pickling-phosphating-saponification treatment is performed. Hydrochloric acid is used for pickling, and the mass fraction of hydrochloric acid is controlled at 10-30%, the temperature is controlled at 20-35°C, and the pickling time t2=247e -c / 6.6 +18; t2 is the pickling time, min; c is the mass fraction of hydrochloric acid during pickling, %;
[0011] The wire heat treatment process comprises the following steps: wire unwinding - scrubbing - electrolytic pickling - online annealing in hydrogen atmosphere - wire winding.
[0012] Furthermore, in the wire rod rolling process, the surface of the forging blank is ground before rolling; the finished wire rod has a diameter of φ8 to 15 mm and a spinning temperature of 800 to 900°C.
[0013] Furthermore, in the solution treatment process, nitrogen is introduced into the heating furnace for protection to ensure that the oxygen content in the furnace is not greater than 0.1%;
[0014] Furthermore, in the solution treatment process, before the wire rod is loaded into the furnace, the heating furnace is preheated first, the temperature is raised to 800-850°C and kept warm for 0.5-1h before loading into the furnace, and the material is kept warm for 1-1.5h; then the temperature is raised to 1130-1150°C within 1-1.5h and kept warm.
[0015] Furthermore, in the solution treatment process, the time from the wire rod being taken out of the furnace to being put into water is ≤40s, and the water temperature before being put into water is not greater than 50°C; the water is taken out after being put into water for 2 minutes, and the water temperature of the water is controlled within 65°C.
[0016] Furthermore, in the wire rod surface treatment step, the wire rod is shot blasted for 10 to 15 minutes.
[0017] Furthermore, in the wire heat treatment process, the electrolytic pickling liquid is sulfuric acid with a concentration of 3-5%, the acid tank temperature is 15-30°C, the ferrous ion concentration is less than 300g / L, the voltage is 5-10V, the current is 20-30A, and the pickling time is 2-3min.
[0018] Furthermore, in the wire heat treatment process, annealing is protected by a hydrogen atmosphere, the concentration ratio of hydrogen to nitrogen in the hydrogen annealing furnace is 2:1 to 3:1, and the annealing temperature is 500 to 600°C.
[0019] The beneficial effects of adopting the above technical solution are:
[0020] 1. Composition design advantages: Based on the traditional low expansion iron-nickel alloy (Invar), the present invention redesigns the C content and the contents of the main alloying elements Cr, Mo, Mn, and Co, while improving the alloy strength, enhancing its hot forming performance, and slowing down the formation of alloy oxide layer during hot working, while ensuring the high electrical conductivity and low thermal expansion coefficient of Invar.
[0021] (1) In the present invention, by adding C, Cr and Mo elements to the alloy, the alloy is solid-solution strengthened and, in combination with the processing method of the present invention, a fine and dispersed second phase is precipitated, thereby improving the strength of the alloy;
[0022] (2) The addition of Cr, Mo, and Si elements can improve the high temperature resistance of the alloy and reduce the thickness of the oxide scale on the alloy surface during the hot working process (forging, hot rolling, heat treatment), thereby improving the overall yield of the material;
[0023] (3) The addition of Cr and Mo elements will increase the thermal expansion coefficient of the alloy. In order to ensure the low expansion characteristics of the alloy without affecting its conductivity, a certain amount of Co element must be added, and the addition amount satisfies: Co = Cr + 0.4Mo ± 0.05, and Co + Ni ≤ 38.6%.
[0024] 2. In the wire rod solid solution process, the nitrogen protection process is used to reduce the oxygen content in the furnace; the heating process is used to ensure that the temperature of the wire rod in the furnace is uniform and meets the solid solution process, while shortening its time in the furnace to the greatest extent and reducing the formation of oxide scale; by controlling the water cooling process after the wire rod is taken out of the furnace, the contact time of the wire rod with the air at high temperature is reduced, the formation of oxide layer is reduced, and the solid solution effect of the wire rod is guaranteed at the same time.
[0025] 3. In the wire rod surface treatment process, the oxide scale can be removed through shot blasting-alkali washing-pickling-phosphating-saponification treatment. Among them, shot blasting can remove loose oxide scale on the surface; in the pickling process, the oxide scale can be fully removed by controlling the acid temperature, concentration and pickling time, and the material loss caused by over-pickling and the hazards such as hydrogen embrittlement and pitting can be avoided.
[0026] 4. In the wire heat treatment process, the scrubbing-electrolytic pickling process can be used to remove the phosphorus saponification layer formed in the wire rod surface treatment process and the drawing powder formed on the surface during the drawing process, and at the same time remove the residual oxide scale on the wire surface; the hydrogen atmosphere in the annealing process can protect the wire from oxidation.
[0027] 5. Through the above-mentioned composition design and production process control, the excellent performance of Invar steel can be ensured while the generation of oxide scale during the hot processing and heat care of wire rods can be reduced to the greatest extent, providing a basis for realizing the production process of non-stripping wire. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the microstructure of the oxide scale on the surface of Invar wire rod after solution treatment under conventional production process;
[0029] Figure 2 This is a microstructure diagram of the oxide scale on the surface of the Invar wire rod after solution treatment in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The chemical composition and mass percentage of the high-strength invar steel wire of the present invention are: C: 0.09-0.32%, Ni: 37.0-38.0%, Mo: 0.3-0.5%, Cr: 0.5-0.7%, Co: 0.6-0.9%, Mn: 0.1-0.3%, Ti≤0.01%, Si: 0.1-0.2%, P≤0.02%, S≤0.01%, and the balance is iron and inevitable impurities; wherein the mass percentage of Cr, Mo, Co and Ni elements satisfies the relationship: Co=Cr+0.4Mo±0.05, and Co+Ni≤38.6%.
[0031] The above-mentioned method for preparing high-strength Invar wire without peeling and with high yield rate is applicable to the production of Invar wire with a diameter of 3.0 to 5.5 mm, including vacuum melting, electroslag refining, forging, wire rod rolling, solution treatment, wire rod surface treatment, wire cold drawing, and wire heat treatment processes; the specific process steps are as follows:
[0032] (1) Vacuum melting process: including raw material preparation, baking and drying, material laying, smelting, steel pouring and demoulding steps.
[0033] (2) Electroslag refining process: including electroslag preparation, electroslag smelting, and electroslag ingot demoulding process.
[0034] (3) Forging process: includes heating, forging and cooling steps.
[0035] (4) Rolling process: After forging, the billet is surface-grinded. The surface and corners of the forged billet are ground with a grinding wheel grinder to remove corner cracks and surface hairlines. Finally, the head of the crack is cut off. Then the continuous rolling mill is used for rolling to φ8-15mm wire rods at a spinning temperature of 800-900℃.
[0036] (5) Solution treatment process: nitrogen is introduced into the heating furnace for protection to ensure that the oxygen content in the furnace is not more than 0.1%; before the wire rod is loaded into the furnace, the heating furnace is preheated first, the temperature is raised to 800-850℃ and kept at this temperature for 0.5-1h before loading into the furnace, and the material is kept at this temperature for 1-1.5h; then the temperature is raised to 1130-1150℃ within 1-1.5h, and the temperature is kept at t1=1.8+0.15D1; then the wire rod is taken out of the furnace and water-cooled, the time from the furnace to the water is ≤40s, and the water temperature before the water is not more than 50℃; the water is taken out 2min after the water is entered, and the outlet water temperature is controlled within 65℃; where t1 is the holding time, h; D1 is the diameter of the wire rod after rolling, mm.
[0037] (6) Wire rod surface treatment process: the wire rod is shot blasted for 10 to 15 minutes, and then alkali-pickling-phosphating-saponification treatment is performed. Hydrochloric acid pickling is used, the mass fraction of hydrochloric acid is controlled at 10 to 30%, the temperature is controlled at 20 to 35°C, and the pickling time t2 = 247e -c / 6.6 +18; t2 is the pickling time, min; c is the mass fraction of hydrochloric acid during pickling, %.
[0038] (7) Wire cold drawing process: The surface reduction rate of the drawing pass is controlled at 20-25%, the drawing speed is not more than 5.5 m / s, and the final diameter of the wire product is 3.0-5.5 mm.
[0039] (8) Wire heat treatment process, the process is wire laying-out-scrubbing-electrolytic pickling-online annealing in hydrogen atmosphere-wire winding. The electrolytic pickling solution is 3-5% sulfuric acid, the acid tank temperature is 15-30°C, the ferrous ion concentration is less than 300g / L, the voltage is 5-10V, the current is 20-30A, and the pickling time is 2-3min. Annealing uses hydrogen atmosphere protection, the concentration ratio of hydrogen:nitrogen in the hydrogen annealing furnace is 2:1-3:1, and the annealing temperature is 500-600°C.
[0040] The chemical composition mass contents of the Invar wires of Examples 1-6 of the present invention are shown in Table 1, the parameter settings of each production process are shown in Table 2-Table 4, and the mechanical properties of the Invar wires are shown in Table 5.
[0041] Table 1. Chemical composition of invar wire in each embodiment.
[0042] Example C Ni Mo Cr Co Mn Ti Si P S 1 0.092 37.9 0.31 0.51 0.62 0.22 0.0086 0.11 0.011 0.003 2 0.18 37.5 0.37 0.62 0.81 0.12 0.0074 0.19 0.013 0.005 3 0.12 37.4 0.49 0.53 0.69 0.28 0.0065 0.17 0.012 0.009 4 0.27 37.6 0.41 0.55 0.75 0.19 0.0095 0.16 0.007 0.005 5 0.31 37.1 0.32 0.67 0.84 0.23 0.0064 0.15 0.019 0.006 6 0.10 37.7 0.47 0.69 0.88 0.17 0.0051 0.18 0.008 0.005
[0043] Table 2. Solution treatment process parameters of various embodiments
[0044]
[0045] Table 3. Rolling and surface treatment process parameters of various embodiments
[0046]
[0047]
[0048] Table 4. Parameters of heat treatment process of wire materials in various embodiments
[0049]
[0050] Table 5 Mechanical properties of invar wires in various embodiments
[0051]
[0052] To illustrate the technical effect of the present invention, Invar wire rods after solution treatment under conventional production process and wire rods after solution treatment in Examples 1-6 of the present invention were taken to test the oxide scale thickness on the wire rod surface and the yield rate. The results are shown in Table 6.
[0053] Table 6. Test results of oxide scale thickness and yield rate on wire rod surface
[0054]
[0055] Figure 1 This is the microstructure of the oxide scale on the surface of Invar wire rod after solution treatment under conventional production process. It can be seen from the figure that the oxide scale has a loose structure and an average thickness of 112μm. In the conventional production process, this oxide scale needs to be removed by mechanical peeling, which seriously affects the yield rate.
[0056] Figure 2 The microstructure of the oxide scale on the surface of the Invar wire rod after solution treatment in Example 1 of the present invention is shown in FIG. 1, and the average oxide scale thickness is 76 μm. Through the subsequent production process in Example 1, the oxide scale can be removed while the yield rate can be greatly improved.
Claims
1. A high-strength invar steel wire material, It is characterized in that Its chemical composition and mass percentage are: C: 0.09-0.32%, Ni: 37.0-38.0%, Mo: 0.3-0.5%, Cr: 0.5-0.7%, Co: 0.6-0.9%, Mn: 0.1-0.3%, Ti≤0.01%, Si: 0.1-0.2%, P≤0.02%, S≤0.01%, and the remainder is iron and inevitable impurities; among which, the mass percentage of Cr, Mo, Co and Ni elements satisfies the relationship: Co=Cr+0.4Mo±0.05, and Co+Ni≤38.6%.
2. The high-strength Invar wire according to claim 1, It is characterized in that The wire has a diameter of 3.0 to 5.5 mm, a tensile strength of ≥1250 MPa, and a thermal expansion coefficient of ≤2.5×10 -6 / ℃, electrical conductivity ≥2%IACS at 20℃.
3. A method for preparing high-strength invar wire without peeling and with high yield rate based on claim 1 or 2, It is characterized in that It includes vacuum melting, electroslag refining, forging, wire rod rolling, solution treatment, wire rod surface treatment, wire cold drawing, and wire heat treatment processes; In the solution treatment process, before the wire rod is loaded into the furnace, the heating furnace is preheated, the temperature is raised to 800-850°C and kept warm before loading into the furnace; then the temperature is raised to 1130-1150°C and kept warm for t 1 =1.8+0.15D 1 ; After that, it is water-cooled; t 1 is the holding time, h; D 1 is the diameter of the wire rod after rolling, mm; In the wire rod surface treatment process, the wire rod is shot blasted, and then alkali-pickling-phosphating-saponification treatment is performed, and hydrochloric acid pickling is used, the mass fraction of hydrochloric acid is controlled at 10-30%, the temperature is controlled at 20-35°C, and the pickling time t 2 =247e -c / 6.6 +18;t 2 is the pickling time, min; c is the mass fraction of hydrochloric acid during pickling, %; The wire heat treatment process comprises the following steps: wire unwinding - scrubbing - electrolytic pickling - online annealing in hydrogen atmosphere - wire winding.
4. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 3, It is characterized in that In the wire rod rolling process, the surface of the forging blank is ground before rolling; the finished wire rod has a diameter of φ8-15 mm and a spinning temperature of 800-900°C.
5. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 4, It is characterized in that In the solution treatment process, nitrogen is introduced into the heating furnace for protection to ensure that the oxygen content in the furnace is not greater than 0.1%.
6. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 5, It is characterized in that In the solution treatment process, before the wire rod is loaded into the furnace, the heating furnace is preheated first, the temperature is raised to 800-850°C and kept warm for 0.5-1h before loading into the furnace, and the material is kept warm for 1-1.5h; then the temperature is raised to 1130-1150°C within 1-1.5h and kept warm.
7. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 6, It is characterized in that In the solution treatment process, the time from the wire rod being taken out of the furnace to being put into water is ≤40s, and the water temperature before being put into water is not higher than 50°C; the water is taken out after being put into water for 2 minutes, and the water temperature of the water is controlled within 65°C.
8. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 7, It is characterized in that In the wire rod surface treatment process, the wire rod is shot blasted for 10 to 15 minutes.
9. The method for preparing high-strength invar wire without peeling and with high yield rate according to any one of claims 1 to 8, It is characterized in that In the wire heat treatment process, the electrolytic pickling liquid is 3-5% sulfuric acid, the acid tank temperature is 15-30°C, the ferrous ion concentration is less than 300g / L, the voltage is 5-10V, the current is 20-30A, and the pickling time is 2-3min.
10. The method for preparing high-strength invar wire without peeling and with high yield rate according to claim 9, It is characterized in that In the wire heat treatment process, annealing is protected by a hydrogen atmosphere, the concentration ratio of hydrogen to nitrogen in the hydrogen annealing furnace is 2:1 to 3:1, and the annealing temperature is 500 to 600°C.