Vitrification agent and preparation method thereof
By using modified silica and composite film-forming agents to form a ceramic protective layer on the metal surface, the environmental pollution problem of phosphating process is solved, and a green ceramic agent with high adhesion and corrosion resistance is achieved, thus improving the coating performance of the metal manufacturing industry.
Patent Information
- Application Number
- CN202411238635.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing phosphating processes cause heavy metal and environmental pollution, and there is a lack of green and environmentally friendly alternatives, making it difficult to maintain good coating adhesion and corrosion resistance in the metal manufacturing industry.
A ceramic coating agent composed of modified silica, composite film-forming agent, composite complexing agent and composite silane coupling agent forms a dense ceramic protective layer on the metal surface through a specific chemical process, thereby improving adhesion and corrosion resistance.
It significantly improves the adhesion, impact resistance and corrosion resistance of the coating, forms a dense ceramic layer, enhances the hardness and stability of the metal surface, resists environmental erosion, and extends service life.
Smart Images

Figure CN119040865A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal treatment agents, and in particular to a ceramic agent and a preparation method thereof. Background Art
[0002] In the metal manufacturing industry, the pre-treatment process for coating is crucial to improving the adhesion and corrosion resistance of the coating. For a long time, phosphating has been the most widely used pre-treatment method for coating. The phosphating film it produces is firmly bonded to the substrate, has a microporous structure, and has good adsorption properties, which can significantly improve the quality of coating. In addition, the phosphating film also has lubricity, insulation and corrosion resistance, so it is widely used in the manufacturing fields of products such as automobiles, machinery manufacturing, aerospace and household appliances. However, the phosphating process is not without drawbacks. It uses phosphoric acid, zinc, manganese and nickel as the main raw materials, which inevitably leads to environmental pollution problems such as heavy metals, phosphorus and nitrite.
[0003] Therefore, people began to actively explore environmentally friendly coating pretreatment processes that can replace traditional phosphating processes. These new processes not only need to maintain the advantages of traditional phosphating processes, such as good coating adhesion and corrosion resistance, but also need to have the advantages of simple process, green environmental protection, and low overall cost. It is in this context that ceramic agents, as a new type of environmentally friendly phosphorus-free conversion agent, came into being.
[0004] The main components of the ceramic agent include zirconium, zirconium titanium, silane, zirconium silane, etc., which can replace phosphating solution and form excellent adhesion and anti-corrosion functions with metal surfaces and subsequent paint coatings. Among them, the effect of the combined use of fluorozirconate and silane coupling agent is particularly significant. During the preparation process of the ceramic agent, by adding special film-forming additives, the metal surfaces such as steel, zinc plate and aluminum are chemically treated to form a mixed insoluble nano-ceramic conversion film. The formation of this conversion film does not require heating, does not produce sediment, and can significantly improve the adhesion and impact resistance of the coating. In summary, how to prepare a ceramic agent that can be better applied to the metal manufacturing industry has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0005] In order to overcome the above technical defects in the prior art, the present invention provides a ceramic agent and a preparation method thereof, aiming to make it better applied in the metal manufacturing industry.
[0006] In order to solve the above technical problems, the technical solutions provided by the present invention are as follows: The embodiment of the present invention discloses a ceramic agent, which is composed of the following components: modified silicon dioxide, a composite film-forming agent component, a composite complexing agent component, a composite silane coupling agent component, deionized water and a hydrochloric acid solution; The modified silicon dioxide is prepared by using silicon dioxide coated with dopamine as a raw material and then modified with a flame retardant; The composite film-forming agent is prepared by mixing hexafluorotitanic acid and hexafluorozirconic acid in equal weight ratios; The composite complexing agent component is prepared by mixing an organic complexing agent and an inorganic complexing agent; The composite silane coupling agent component is prepared by mixing multiple silane coupling agents.
[0007] Furthermore, the preparation method of the dopamine-coated silica is: S2.1, pour 0.7g of nano-silicon dioxide into 100mL Tris-HCl buffer, and the result after ultrasonic dispersion is recorded as the silicon dioxide component, pour 1.4g of dopamine hydrochloride into 200mL Tris-HCl buffer, and the result after stirring and dispersion is recorded as the dopamine hydrochloride component; S2.2. Pour the silica component into the dopamine hydrochloride component for ultrasonic treatment, then place it in a 25°C water bath and stir at 180 r / min for 12-24 hours to react. After the reaction is completed, the precipitated product is centrifuged and washed with deionized water and freeze-dried. After grinding through a 200-mesh sieve, the resulting product is dopamine-coated silica.
[0008] Furthermore, the preparation method of the Tris-HCl buffer in S2.1 is: to a Tris solution with a concentration of 0.01 mol / L, a hydrochloric acid solution with a mass fraction of 10% is added to adjust the pH value to 4, and the result is a Tris-HCl buffer. The specific operation of ultrasonic dispersion in S2.1 is ultrasonic dispersion at a frequency of 28 kHz for 30 minutes, and the specific operation of stirring dispersion in S2.1 is stirring at a speed of 500 r / min for 30 minutes.
[0009] Furthermore, the specific operation of ultrasonic treatment in S2.2 is ultrasonic dispersion at a frequency of 26 kHz for 15 minutes, and the specific operation of centrifugal cleaning in S2.2 is: first use deionized water as a washing liquid, centrifuge at a speed of 8000 r / min for 15 minutes to retain the precipitate, and then use deionized water as a washing liquid, centrifuge at a speed of 8000 r / min for 10 minutes to retain the precipitate.
[0010] Furthermore, the preparation method of the modified silicon dioxide is: S5.1. Pour 0.5 g of dopamine-coated silica, 0.3 g of phosphorus oxychloride and 50 mL of tetrahydrofuran into a flask, add 0.25 g of triethylamine and perform ultrasonic treatment at 25°C. The result is recorded as the reaction component. S5.2. Dissolve 0.7 g of 4,4-diaminodiphenylmethane in 20 mL of tetrahydrofuran, then drip it into the reaction components at a drip rate of 1 drop / s, let it stand at room temperature for 24 hours to react to obtain product components, purify the product components with tetrahydrofuran and deionized water in turn, and then dry them to obtain modified silica.
[0011] Furthermore, the specific operation of the ultrasonic treatment in S5.1 is ultrasonic dispersion at a frequency of 23 kHz for 1 hour, and the specific operation of the drying treatment in S5.2 is drying under reduced pressure at a temperature of 80° C. for 24 hours.
[0012] Furthermore, the preparation method of the composite complexing agent component is: ethylenediaminetetraacetic acid, sodium tartrate, sodium tripolyphosphate, sodium pyrophosphate and sodium hexametaphosphate are weighed in a weight ratio of 5:3:1:2:1, poured into a ball mill for ball milling, and the resultant is the composite complexing agent component after ball milling at a speed of 800r / min for 10 minutes.
[0013] Furthermore, the preparation method of the composite silane coupling agent component is: silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570 are measured in a volume ratio of 1:2:3 and poured into a flask, and stirred at a speed of 500r / min for 10 minutes to obtain the composite silane coupling agent component.
[0014] In a second aspect, a method for preparing a ceramic agent comprises the following steps: Step 1, weighing 1g of modified silica and 1-2g of a composite silane coupling agent component, pouring them into a ball mill and ball milling them, and the obtained components are recorded as ball milling components; Step 2, weigh 2-3g of the composite film-forming agent component and add it to 600mL of deionized water, stir and disperse, then add 2-3g of the composite complexing agent component and the ball milling component, disperse evenly, add deionized water to make the volume to 1L, and the result is recorded as the fixed volume component; Step 3: Add 10% by mass hydrochloric acid solution to the fixed volume component to adjust the pH value to 5, and the obtained product is the ceramic agent.
[0015] Furthermore, the specific operation of ball milling in step 1 is ball milling at a speed of 800r / min for 10min, the specific operation of stirring and dispersing in step 2 is stirring at a speed of 400r / min for 10min, and the specific operation of uniform dispersion in step 2 is stirring at a speed of 300r / min for 10min.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a ceramic agent and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses polydopamine-coated silicon dioxide, phosphorus oxychloride and 4,4-diaminodiphenylmethane as raw materials to prepare polydopamine-coated silicon dioxide modified with a flame retardant, and adds the polydopamine-coated silicon dioxide as an additive to a film-forming agent to prepare a ceramic material, which can significantly improve the flame retardancy, stability, film-forming performance and ceramic effect of the ceramic material; polydopamine is a polymer with excellent biocompatibility and adhesion, and its coating layer can be firmly attached to the surface of silicon dioxide to form a protective layer, which not only enhances the wear resistance, weather resistance and chemical stability of silicon dioxide, but also can prevent the interaction between silicon dioxide and other components to a certain extent, thereby maintaining the overall stability of the material; secondly, the flame retardant-modified polydopamine is coated with Adding silica as an additive to the film-forming agent can significantly improve the film-forming properties of the film-forming agent. This additive can serve as a filler or reinforcing agent in the film-forming process to improve the performance indicators of the film-forming agent such as viscosity, adhesion and hardness. At the same time, its uniform dispersion also helps to form a smoother and denser film layer. Finally, ceramicization refers to the process of forming a hard protective layer similar to ceramic on the surface of a material through a specific chemical or physical process. Adding flame retardant-modified polydopamine-coated silica as an additive to the ceramicizer can accelerate the ceramicization process and enhance the ceramicization effect. This additive can serve as a nucleating agent or catalyst to promote the formation of a denser and harder ceramic layer on the surface of the material, thereby improving the wear resistance, corrosion resistance and high temperature resistance of the material.
[0017] 2. The ceramic agent prepared by using hexafluorotitanic acid and hexafluorozirconic acid as film-forming agents, and using complexing agents and silane coupling agents as additives has excellent film-forming performance, corrosion resistance, surface performance, environmental protection and process flexibility; hexafluorotitanic acid and hexafluorozirconic acid as film-forming agents can form a dense oxide film on the metal surface, which can not only effectively isolate air and moisture and prevent metal corrosion, but also improve the hardness and wear resistance of the metal surface. The addition of complexing agents can promote the combination between the film layer and the metal substrate and enhance the adhesion of the film, which makes the ceramic film more firmly bonded. It adheres to the metal surface and is not easy to fall off; secondly, the oxide film formed by hexafluorotitanic acid and hexafluorozirconic acid has excellent chemical stability and can resist the erosion of various acids, alkalis and salt solutions, which enables the metal workpiece to maintain good performance in harsh environments. The ceramic film also has good weather resistance and can resist the erosion of natural factors such as ultraviolet rays, high temperature and humidity, which helps to extend the service life of the metal workpiece; the addition of silane coupling agent can improve the surface finish of the ceramic film, making it smoother and more delicate, which helps to improve the appearance quality and touch of the metal workpiece. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings are used for further understanding of the present invention and are used to explain the present invention together with the embodiments of the present invention, but do not constitute a limitation of the present invention.
[0019] Figure 1 It is a table diagram of test data of embodiments of the present invention and comparative examples. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] The present invention will be further described below in conjunction with the embodiments. Example 1
[0022] A ceramic agent of this embodiment, the ceramic agent is composed of the following components: modified silicon dioxide, a composite film-forming agent component, a composite complexing agent component, a composite silane coupling agent component, deionized water and a hydrochloric acid solution; Modified silica is prepared by using dopamine-coated silica as raw material and then modified with a flame retardant; Wherein, the preparation method of dopamine-coated silica is: S2.1, 0.7g of nano-silicon dioxide was poured into 100mL of Tris-HCl buffer, and the mixture was ultrasonically dispersed at a frequency of 28kHz for 30min, and the result was recorded as the silicon dioxide component. 1.4g of dopamine hydrochloride was poured into 200mL of Tris-HCl buffer, and the mixture was stirred at a speed of 500r / min for 30min, and the result was recorded as the dopamine hydrochloride component. The preparation method of the Tris-HCl buffer was as follows: a hydrochloric acid solution with a mass fraction of 10% was added dropwise to a Tris solution with a concentration of 0.01mol / L to adjust the pH value to 4, and the result was the Tris-HCl buffer; S2.2. Pour the silica component into the dopamine hydrochloride component and disperse it ultrasonically at a frequency of 26kHz for 15 minutes, then place it in a water bath at 25°C and stir it at a speed of 180r / min for 12 hours to react. After the reaction is completed, the precipitated product is centrifuged and washed with deionized water and freeze-dried. After grinding through a 200-mesh sieve, the resulting dopamine-coated silica is obtained. The specific operation of centrifugal washing is: first use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 15 minutes to retain the precipitate, and then use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 10 minutes to retain the precipitate.
[0023] The preparation method of modified silicon dioxide is: S5.1. Pour 0.5 g dopamine-coated silica, 0.3 g phosphorus oxychloride and 50 mL tetrahydrofuran into a flask, add 0.25 g triethylamine and disperse by ultrasound at 25°C and 23 kHz for 1 h. The obtained product is recorded as the reaction component. S5.2. Dissolve 0.7 g of 4,4-diaminodiphenylmethane in 20 mL of tetrahydrofuran, then drip it into the reaction components at a drip rate of 1 drop / s, let it stand at room temperature for 24 hours to react to obtain product components, purify the product components with tetrahydrofuran and deionized water in turn, and then dry them at 80°C under reduced pressure for 24 hours to obtain modified silica.
[0024] The composite film-forming agent component is prepared by mixing hexafluorotitanic acid and hexafluorozirconic acid in an equal weight ratio. The preparation method is as follows: ethylenediaminetetraacetic acid, sodium tartrate, sodium tripolyphosphate, sodium pyrophosphate and sodium hexametaphosphate are weighed in a weight ratio of 5:3:1:2:1, poured into a ball mill for ball milling, and the resultant is a composite complexing agent component after ball milling at a speed of 800r / min for 10 minutes.
[0025] The composite complexing agent component is prepared by mixing an organic complexing agent and an inorganic complexing agent; The composite silane coupling agent component is prepared by mixing a plurality of silane coupling agents, and the preparation method is as follows: silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570 are measured in a volume ratio of 1:2:3 and poured into a flask, and stirred at a speed of 500 r / min for 10 minutes to obtain the composite silane coupling agent component.
[0026] A method for preparing a ceramic agent, the method comprising the following steps: Step 1, weighing 1g of modified silica and 1g of composite silane coupling agent components, pouring them into a ball mill and ball milling them at a speed of 800r / min for 10min, and the obtained components are recorded as ball milling components; Step 2, weigh 2g of the composite film-forming agent component and add it to 600mL of deionized water, stir at a speed of 400r / min for 10min, then add 2g of the composite complexing agent component and the ball milling component, stir at a speed of 300r / min for 10min, then add deionized water to make the volume to 1L, and the obtained volume is recorded as the fixed volume component; Step 3: Add 10% by mass hydrochloric acid solution to the fixed volume component to adjust the pH value to 5, and the obtained product is the ceramic agent. Example 2
[0027] A ceramic agent of this embodiment, the ceramic agent is composed of the following components: modified silicon dioxide, a composite film-forming agent component, a composite complexing agent component, a composite silane coupling agent component, deionized water and a hydrochloric acid solution; Modified silica is prepared by using dopamine-coated silica as raw material and then modified with a flame retardant; Wherein, the preparation method of dopamine-coated silica is: S2.1, 0.7g of nano-silicon dioxide was poured into 100mL of Tris-HCl buffer, and the mixture was ultrasonically dispersed at a frequency of 28kHz for 30min, and the result was recorded as the silicon dioxide component. 1.4g of dopamine hydrochloride was poured into 200mL of Tris-HCl buffer, and the mixture was stirred at a speed of 500r / min for 30min, and the result was recorded as the dopamine hydrochloride component. The preparation method of the Tris-HCl buffer was as follows: a hydrochloric acid solution with a mass fraction of 10% was added dropwise to a Tris solution with a concentration of 0.01mol / L to adjust the pH value to 4, and the result was the Tris-HCl buffer; S2.2. Pour the silica component into the dopamine hydrochloride component and disperse it ultrasonically at a frequency of 26kHz for 15 minutes, then place it in a water bath at 25°C and stir it at a speed of 180r / min for 24 hours to react. After the reaction is completed, the precipitated product is centrifuged and washed with deionized water and freeze-dried. After grinding through a 200-mesh sieve, the resulting dopamine-coated silica is obtained. The specific operation of centrifugal washing is: first use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 15 minutes to retain the precipitate, and then use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 10 minutes to retain the precipitate.
[0028] The preparation method of modified silicon dioxide is: S5.1. Pour 0.5 g dopamine-coated silica, 0.3 g phosphorus oxychloride and 50 mL tetrahydrofuran into a flask, add 0.25 g triethylamine and disperse by ultrasound at 25°C and 23 kHz for 1 h. The obtained product is recorded as the reaction component. S5.2. Dissolve 0.7 g of 4,4-diaminodiphenylmethane in 20 mL of tetrahydrofuran, then drip it into the reaction components at a drip rate of 1 drop / s, let it stand at room temperature for 24 hours to react to obtain product components, purify the product components with tetrahydrofuran and deionized water in turn, and then dry them at 80°C under reduced pressure for 24 hours to obtain modified silica.
[0029] The composite film-forming agent component is prepared by mixing hexafluorotitanic acid and hexafluorozirconic acid in an equal weight ratio. The preparation method is as follows: ethylenediaminetetraacetic acid, sodium tartrate, sodium tripolyphosphate, sodium pyrophosphate and sodium hexametaphosphate are weighed in a weight ratio of 5:3:1:2:1, poured into a ball mill for ball milling, and the resultant is a composite complexing agent component after ball milling at a speed of 800r / min for 10 minutes.
[0030] The composite complexing agent component is prepared by mixing an organic complexing agent and an inorganic complexing agent; The composite silane coupling agent component is prepared by mixing a plurality of silane coupling agents, and the preparation method is as follows: silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570 are measured in a volume ratio of 1:2:3 and poured into a flask, and stirred at a speed of 500 r / min for 10 minutes to obtain the composite silane coupling agent component.
[0031] A method for preparing a ceramic agent, the method comprising the following steps: Step 1, weighing 1g of modified silica and 2g of a composite silane coupling agent component, pouring them into a ball mill and ball milling them at a speed of 800r / min for 10min, and the obtained components are recorded as ball milling components; Step 2, weigh 3g of the composite film-forming agent component and add it to 600mL of deionized water, stir at a speed of 400r / min for 10min, then add 3g of the composite complexing agent component and the ball milling component, stir at a speed of 300r / min for 10min, then add deionized water to make the volume to 1L, and the result is recorded as the fixed volume component; Step 3: Add 10% by mass hydrochloric acid solution to the fixed volume component to adjust the pH value to 5, and the obtained product is the ceramic agent. Example 3
[0032] A ceramic agent of this embodiment, the ceramic agent is composed of the following components: modified silicon dioxide, a composite film-forming agent component, a composite complexing agent component, a composite silane coupling agent component, deionized water and a hydrochloric acid solution; Modified silica is prepared by using dopamine-coated silica as raw material and then modified with a flame retardant; Wherein, the preparation method of dopamine-coated silica is: S2.1, 0.7g of nano-silicon dioxide was poured into 100mL of Tris-HCl buffer, and the mixture was ultrasonically dispersed at a frequency of 28kHz for 30min, and the result was recorded as the silicon dioxide component. 1.4g of dopamine hydrochloride was poured into 200mL of Tris-HCl buffer, and the mixture was stirred at a speed of 500r / min for 30min, and the result was recorded as the dopamine hydrochloride component. The preparation method of the Tris-HCl buffer was as follows: a hydrochloric acid solution with a mass fraction of 10% was added dropwise to a Tris solution with a concentration of 0.01mol / L to adjust the pH value to 4, and the result was the Tris-HCl buffer; S2.2. Pour the silica component into the dopamine hydrochloride component and disperse it ultrasonically at a frequency of 26kHz for 15 minutes, then place it in a water bath at 25°C and stir it at a speed of 180r / min for 36 hours to react. After the reaction is completed, the precipitated product is centrifuged and washed with deionized water and freeze-dried. After grinding through a 200-mesh sieve, the resulting dopamine-coated silica is obtained. The specific operation of centrifugal washing is: first use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 15 minutes to retain the precipitate, and then use deionized water as a washing liquid, centrifuge at a speed of 8000r / min for 10 minutes to retain the precipitate.
[0033] The preparation method of modified silicon dioxide is: S5.1. Pour 0.5 g dopamine-coated silica, 0.3 g phosphorus oxychloride and 50 mL tetrahydrofuran into a flask, add 0.25 g triethylamine and disperse by ultrasound at 25°C and 23 kHz for 1 h. The obtained product is recorded as the reaction component. S5.2. Dissolve 0.7 g of 4,4-diaminodiphenylmethane in 20 mL of tetrahydrofuran, then drip it into the reaction components at a drip rate of 1 drop / s, let it stand at room temperature for 24 hours to react to obtain product components, purify the product components with tetrahydrofuran and deionized water in turn, and then dry them at 80°C under reduced pressure for 24 hours to obtain modified silica.
[0034] The composite film-forming agent component is prepared by mixing hexafluorotitanic acid and hexafluorozirconic acid in an equal weight ratio. The preparation method is as follows: ethylenediaminetetraacetic acid, sodium tartrate, sodium tripolyphosphate, sodium pyrophosphate and sodium hexametaphosphate are weighed in a weight ratio of 5:3:1:2:1, poured into a ball mill for ball milling, and the resultant is a composite complexing agent component after ball milling at a speed of 800r / min for 10 minutes.
[0035] The composite complexing agent component is prepared by mixing an organic complexing agent and an inorganic complexing agent; The composite silane coupling agent component is prepared by mixing a plurality of silane coupling agents, and the preparation method is as follows: silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570 are measured in a volume ratio of 1:2:3 and poured into a flask, and stirred at a speed of 500 r / min for 10 minutes to obtain the composite silane coupling agent component.
[0036] A method for preparing a ceramic agent, the method comprising the following steps: Step 1, weighing 1g of modified silica and 2g of a composite silane coupling agent component, pouring them into a ball mill and ball milling them at a speed of 800r / min for 10min, and the obtained components are recorded as ball milling components; Step 2, weigh 2g of the composite film-forming agent component and add it to 600mL of deionized water, stir at a speed of 400r / min for 10min, then add 3g of the composite complexing agent component and the ball milling component, stir at a speed of 300r / min for 10min, then add deionized water to make the volume to 1L, and the result is recorded as the fixed volume component; Step 3: Add 10% by mass hydrochloric acid solution to the fixed volume component to adjust the pH value to 5, and the obtained product is the ceramic agent.
[0037] Comparative Example 1: The ceramic agent and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the modified silicon dioxide in Example 1 is replaced by nano silicon dioxide.
[0038] Comparative Example 2: The ceramic agent and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 2, the composite film-forming agent component in Example 1 is replaced with hexafluorozirconic acid.
[0039] Comparative Example 3: The ceramic agent and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 3, the composite complexing agent component in Example 1 is replaced with ethylenediaminetetraacetic acid.
[0040] Comparative Example 4: The ceramic agent and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 4, the composite silane coupling agent component in Example 1 is replaced with the silane coupling agent KH-560.
[0041] Performance Test: The aluminum alloy was immersed in the ceramics in Examples 1-3 and Comparative Examples 1-4 by chemical immersion method for film-forming treatment. The obtained samples were marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-4 was tested.
[0042] 1. The salt spray corrosion resistance of the membrane was tested using a LYW-150 salt spray box. The experimental solution was a 5% NaCl aqueous solution. The pH value of the solution was adjusted to 7 using Na2CO3. The temperature in the box was 35°C. The sample was placed at 20° to the vertical direction. Continuous spraying was used. The spray volume per 80cm2 was controlled at 1-2mL / h. The salt spray corrosion method was used to evaluate the corrosion resistance of the membrane based on the 12h corrosion area on the membrane surface. The corrosion area data was recorded in Figure 1 ; 2. The copper sulfate drip method is used to carry out the drip corrosion resistance test. The composition of each liter of drip solution is: 41gCuSO4·5H2O, 35g sodium chloride, and 13ml hydrochloric acid solution with a concentration of 0.1mol / L. Three drops are dripped on each surface of the sample. The shortest time for the drip solution on the surface of the sample to change from sky blue to yellow or light red is the corrosion resistance time. The obtained drip corrosion resistance time data is recorded in Figure 1 ; 3. The bonding strength of the film layer is measured according to GB / T9791-2003 "Test method for chromate conversion coating of zinc, aluminum-zinc alloy and zinc-aluminum alloy". The bonding strength is divided into three levels: Ⅰ, Ⅱ and Ⅲ. Ⅰ means strong bonding, Ⅱ means qualified bonding, Ⅲ means poor bonding. The data are recorded in Figure 1 .
[0043] pass Figure 1 The data show that the aluminum alloy surface treated with the ceramic film in Examples 1-3 has better corrosion resistance, stronger surface bonding force, and smaller corrosion area after 12 hours than the aluminum alloy surface treated with the ceramic film in Comparative Examples 1-4, which indicates that the modified silica, composite film-forming agent component, composite complexing agent component, and composite silane coupling agent component added to the ceramic can improve the performance of the ceramic.
[0044] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0045] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A ceramic agent, characterized in that: The ceramic agent is composed of the following components: modified silicon dioxide, a composite film-forming agent component, a composite complexing agent component, a composite silane coupling agent component, deionized water and hydrochloric acid solution; The modified silicon dioxide is prepared by using silicon dioxide coated with dopamine as a raw material and then modified with a flame retardant; The composite film-forming agent is prepared by mixing hexafluorotitanic acid and hexafluorozirconic acid in equal weight ratios; The composite complexing agent component is prepared by mixing an organic complexing agent and an inorganic complexing agent; The composite silane coupling agent component is prepared by mixing multiple silane coupling agents.
2. A ceramic agent according to claim 1, characterized in that: The preparation method of the dopamine-coated silica is: S2.1, pour 0.7g of nano-silicon dioxide into 100mL Tris-HCl buffer, and the result after ultrasonic dispersion is recorded as the silicon dioxide component, pour 1.4g of dopamine hydrochloride into 200mL Tris-HCl buffer, and the result after stirring and dispersion is recorded as the dopamine hydrochloride component; S2.
2. Pour the silica component into the dopamine hydrochloride component for ultrasonic treatment, then place it in a 25°C water bath and stir at 180 r / min for 12-24 hours to react. After the reaction is completed, the precipitated product is centrifuged and washed with deionized water and freeze-dried. After grinding through a 200-mesh sieve, the resulting product is dopamine-coated silica.
3. A ceramic agent according to claim 2, characterized in that: The preparation method of Tris-HCl buffer in S2.1 is: to a Tris solution with a concentration of 0.01 mol / L, a hydrochloric acid solution with a mass fraction of 10% is added to adjust the pH value to 4, and the result is Tris-HCl buffer. The specific operation of ultrasonic dispersion in S2.1 is ultrasonic dispersion at a frequency of 28 kHz for 30 minutes, and the specific operation of stirring dispersion in S2.1 is stirring at a speed of 500 r / min for 30 minutes.
4. A ceramic agent according to claim 2, characterized in that: The specific operation of ultrasonic treatment in S2.2 is ultrasonic dispersion at a frequency of 26kHz for 15 minutes. The specific operation of centrifugal cleaning in S2.2 is: first use deionized water as the washing liquid, centrifuge at a speed of 8000r / min for 15 minutes to retain the precipitate, and then use deionized water as the washing liquid, centrifuge at a speed of 8000r / min for 10 minutes to retain the precipitate.
5. A ceramic agent according to claim 1, characterized in that: The preparation method of the modified silicon dioxide is: S5.
1. Pour 0.5 g of dopamine-coated silica, 0.3 g of phosphorus oxychloride and 50 mL of tetrahydrofuran into a flask, add 0.25 g of triethylamine and perform ultrasonic treatment at 25°C. The result is recorded as the reaction component. S5.
2. Dissolve 0.7 g of 4,4-diaminodiphenylmethane in 20 mL of tetrahydrofuran, then drip it into the reaction components at a drip rate of 1 drop / s, let it stand at room temperature for 24 hours to react to obtain product components, purify the product components with tetrahydrofuran and deionized water in turn, and then dry them to obtain modified silica.
6. A ceramic agent according to claim 5, characterized in that: The specific operation of the ultrasonic treatment in S5.1 is ultrasonic dispersion at a frequency of 23 kHz for 1 hour, and the specific operation of the drying treatment in S5.2 is drying under reduced pressure at a temperature of 80° C. for 24 hours.
7. A ceramic agent according to claim 1, characterized in that: The preparation method of the composite complexing agent component is as follows: ethylenediaminetetraacetic acid, sodium tartrate, sodium tripolyphosphate, sodium pyrophosphate and sodium hexametaphosphate are weighed in a weight ratio of 5:3:1:2:1, poured into a ball mill for ball milling, and the resultant is the composite complexing agent component after ball milling at a speed of 800 r / min for 10 minutes.
8. A ceramic agent according to claim 1, characterized in that: The preparation method of the composite silane coupling agent component is: silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570 are measured in a volume ratio of 1:2:3, poured into a flask, and stirred at a speed of 500 r / min for 10 minutes to obtain the composite silane coupling agent component.
9. A method for preparing a ceramic agent according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: Step 1, weighing 1g of modified silica and 1-2g of a composite silane coupling agent component, pouring them into a ball mill and ball milling them, and the obtained components are recorded as ball milling components; Step 2, weigh 2-3g of the composite film-forming agent component and add it to 600mL of deionized water, stir and disperse, then add 2-3g of the composite complexing agent component and the ball milling component, disperse evenly, add deionized water to make the volume to 1L, and the result is recorded as the fixed volume component; Step 3: Add 10% by mass hydrochloric acid solution to the fixed volume component to adjust the pH value to 5, and the obtained product is the ceramic agent.
10. The method for preparing a ceramic agent according to claim 9, characterized in that: The specific operation of ball milling in step 1 is ball milling at a speed of 800 r / min for 10 min, the specific operation of stirring and dispersing in step 2 is stirring at a speed of 400 r / min for 10 min, and the specific operation of uniform dispersion in step 2 is stirring at a speed of 300 r / min for 10 min.
Citation Information
Cited By
Phosphate composite flame retardant and preparation method thereof
CN119708639A