Active cathode for electrolytic chlorine production and preparation method thereof

By forming a nano-sized alloy film of platinum and lanthanum on a titanium mesh, combined with plasma cleaning technology, the problem of easy corrosion of cathode materials and high hydrogen evolution overpotential is solved, and the electrolytic chlorine-made cathode with low energy consumption and long life is achieved, suitable for the chlor-alkali industry and other fields.

CN119040931APending Publication Date: 2024-11-29JIANGXI STANDE ELECTRODE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124879.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29

Smart Images

  • Figure CN119040931A_ABST
    Figure CN119040931A_ABST
Patent Text Reader

Abstract

The invention discloses an active cathode for electrolytic chlorine production and a preparation method thereof, and belongs to the technical field of electrolytic chlorine production, and the active cathode comprises a titanium mesh, and a middle layer and an activation layer which are attached to the titanium mesh. The preparation method comprises the following steps: by taking a titanium mesh as a matrix, carrying out sand blasting and etching on the titanium mesh to form a rough surface on the titanium mesh; uniformly coating the pretreated titanium mesh with a platinum compound solution, and performing high-temperature sintering to form an intermediate layer; and coating the intermediate layer with a mixed solution of ruthenium trichloride and a lanthanum compound, and performing high-temperature sintering to form the activation layer. The middle layer is mainly platinum dioxide, so that the titanium surface can be prevented from being oxidized, and the conductivity of the electrode is improved; the activation layer is mainly ruthenium dioxide, and rare earth element lanthanum is introduced, so that the hydrogen evolution overpotential of the cathode can be reduced, and the durability is improved. The active cathode prepared by the invention has relatively low hydrogen evolution overpotential and relatively long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention mainly relates to the technical field of electrolytic chlorine production, and specifically relates to an active cathode for electrolytic chlorine production and a preparation method thereof. Background Art

[0002] Electrolytic chlorine production includes chlor-alkali industry, chlorate production and hypochlorite production. Since the 1960s and 1970s, energy-saving anodes have been widely used. However, the high energy consumption caused by the high overpotential on the cathode still restricts the development of these fields. At the same time, due to the development of ion membrane technology, new requirements are also put forward for the cathode in terms of process. In addition, under high alkali concentration, conventional cathode materials such as low-carbon steel are easily corroded and cannot meet the requirements of long-term stable electrolysis.

[0003] Although titanium cathode has the advantages of excellent corrosion resistance and long service life, it can easily penetrate into the matrix and cause hydrogen embrittlement when it is used as cathode during electrolysis. At the same time, titanium has weak catalytic activity, high overpotential as cathode, and high energy consumption. In addition, when shut down, titanium is easily oxidized to form a layer of dense titanium dioxide with high resistance value on the surface, and its decreased conductivity will further increase energy consumption.

[0004] At present, the metal or alloy electrodes such as low carbon steel, titanium, nickel, etc. commonly used in the field of electrolytic chlorine production have a hydrogen evolution overpotential of more than 300mV. It is necessary to develop and design a cathode with low hydrogen evolution overpotential and long service life. Summary of the invention

[0005] The technical solution of the present invention aims at the technical problem that the existing technical solutions are too single, and provides a solution that is significantly different from the existing technologies. It mainly provides an active cathode for electrolytic chlorine production and a preparation method thereof, so as to meet the requirements of cathode materials with low hydrogen evolution overpotential and long service life.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: A method for preparing an active cathode for electrolytic chlorine production comprises the following steps: S1. Substrate pretreatment: using the titanium mesh as the substrate, sandblasting and etching it to form a rough surface of the titanium mesh; S2, preparing the intermediate layer: uniformly coating the platinum compound solution on the pretreated titanium mesh, and sintering at a high temperature to form the intermediate layer; S3. Preparation of an activation layer: coating a mixed solution of ruthenium trichloride and lanthanum compound on the intermediate layer, and forming an activation layer through high-temperature sintering.

[0007] Specifically, in step S1, after sandblasting, the surface roughness of the titanium mesh is: Ra>5 μm, Rz>30 μm.

[0008] Specifically, in step S1, the etching is: immersing the titanium mesh in an inorganic acid solution (such as hydrochloric acid, oxalic acid, sulfuric acid, etc.) at 80-110° C. for more than 10 minutes, rinsing with pure water after immersion, and then drying.

[0009] Specifically, in step S2, in the platinum compound solution, the platinum compound is at least one of chloroplatinic acid and hydroxyplatinic acid, the solvent used is an alcohol solution (such as isopropanol, butanol, etc.), and the platinum content is 0.1-0.5 g / L.

[0010] Specifically, in step S2, the high temperature sintering temperature is 400-600°C, the sintering time is greater than 20 min, and the coating and sintering are repeated 2-5 times, so that the thickness of the deposited intermediate layer is 100-500 nm. At a temperature of 400-600°C, the oxides of platinum and titanium are both rutile crystals and can form an alloy. Repeated sintering has better bonding strength than single sintering.

[0011] Specifically, in step S3, in the mixed solution of ruthenium trichloride and lanthanum compound, the lanthanum compound is at least one of lanthanum nitrate and lanthanum carbonate, the solvent used is hydrochloric acid or an alcohol solution (such as ethylene glycol, isopropanol, butanol, etc.), and the ratio of ruthenium to lanthanum is 3:1-10:1.

[0012] Specifically, in step S3, the high temperature sintering temperature is 420-550°C, the sintering time is greater than 30 min, and the coating and sintering are repeated 4-10 times to make the thickness of the deposited activation layer 0.5-3 μm.

[0013] Furthermore, in steps S2 and S3, before the first coating, the titanium mesh is placed in a plasma cleaner for cleaning and activation.

[0014] Specifically, the cleaning activation is performed in an inert gas (eg, nitrogen, argon, etc.) chamber, the discharge power is greater than 10 MHz, and the processing time is 0.4-5 min.

[0015] The present invention also provides an active cathode for electrolytic chlorine production, the active cathode comprising a titanium mesh and an intermediate layer and an activation layer attached to the titanium mesh; the active cathode is prepared by the above preparation method.

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses titanium as the substrate, which has good corrosion resistance. The titanium mesh is then sandblasted and etched. Sandblasting can improve the surface roughness of the titanium mesh, and etching can remove oxides on the substrate surface and form a porous morphology. Both can increase the specific surface area of ​​the electrode to reduce the actual current density of the electrode, thereby reducing the overpotential of hydrogen evolution. At the same time, the surface of the substrate has a certain degree of roughness, which can improve the bonding force between the intermediate layer and the activation layer, thereby increasing the service life.

[0017] (2) The present invention coats and sintered platinum compounds on the surface of the titanium substrate. The oxides of platinum and titanium at 400-600 °C are both rutile crystals. The lattice constants of rutile titanium dioxide and platinum dioxide are both a=4.593 Å and c=2.9582 Å. In the process of preparing the platinum dioxide intermediate layer on the titanium mesh surface by thermal decomposition, a nanometer-sized titanium dioxide and platinum dioxide alloy film is formed on the titanium surface. On the one hand, it can avoid the direct formation of titanium dioxide with very poor conductivity (to prevent titanium oxidation). At the same time, it can prevent the hydrogen precipitated from the cathode during the electrolysis reaction from entering the interior of the titanium substrate and solve the problem of hydrogen embrittlement caused by hydrogen infiltration into the substrate, thereby improving the durability and service life of the substrate; on the other hand, the intermediate layer plays a transitional role to improve the bonding force of the catalytic layer, which is not easy to fall off during electrolysis, thereby improving the service life. In addition, platinum has excellent conductivity, which makes the titanium cathode have better conductivity, and can reduce the internal resistance of the cathode when the electrolysis is powered, thereby reducing the cell voltage and reducing power consumption.

[0018] (3) The present invention coats and sinters ruthenium trichloride and lanthanum compounds on the intermediate layer to form ruthenium dioxide and lanthanum salts, wherein platinum and ruthenium belong to the platinum group of precious metals and have very close atomic radii. The activation layer of ruthenium dioxide prepared on the platinum dioxide intermediate layer has good bonding strength, and the activation layer is not easy to fall off during electrolysis and has better durability. Ruthenium dioxide has excellent electrocatalytic performance and alkali corrosion resistance in alkaline electrolytes, and the surface of ruthenium dioxide contains a large number of active sites, which can effectively adsorb hydrogen ions (H+) and promote the generation reaction of hydrogen; under alkaline conditions, hydroxyl groups (-OH) are formed on the surface of ruthenium dioxide, and these hydroxyl groups can participate in the generation process of hydrogen as intermediates, reducing the hydrogen evolution overpotential; ruthenium dioxide usually has a large specific surface area, which provides more catalytic active centers, thereby reducing the hydrogen evolution overpotential, so that the cathode activation layer has a significantly lower hydrogen evolution overpotential. Lanthanum is the most alkaline metal and has a certain catalytic activity. The addition of lanthanum turns the homogeneous ruthenium dioxide coating into a two-phase coating. The thermal expansion coefficients of the two substances are different, resulting in the surface morphology in the form of mud cracks after high-temperature sintering and cooling. The existence of these mud cracks is conducive to the release of hydrogen gas at the cathode. In addition, the existence of mud cracks can increase the specific surface area of ​​the coating, reduce the real current density during electrolysis, and achieve the effect of reducing the overpotential of hydrogen evolution. At the same time, the introduction of lanthanum can reduce the exposed sites of ruthenium dioxide, and lanthanum has better alkali corrosion resistance than ruthenium, so it can enhance the stability of the activation layer and thus increase the service life.

[0019] (4) The intermediate layer in the present invention uses a platinum compound. Among all the "electrocatalysts" that may promote the key chemical reaction (oxygen reduction reaction or ORR), platinum is by far the best. However, platinum will quickly degrade after a small number of cycles in a highly corrosive electrolyte environment. The present invention introduces lanthanum into the activation layer, and after plasma activation and high-temperature sintering, a platinum-lanthanum oxide alloy is formed on the surface of the intermediate layer platinum dioxide, which can improve the stability of platinum.

[0020] (5) The present invention performs a plasma cleaning before each coating and sintering. A high-energy disordered plasma is generated under a certain pressure by a radio frequency power supply. The active particles and high-energy rays contained in the plasma react and collide with the surface organic pollutant molecules to form small molecular volatile substances, which are removed from the surface. On the one hand, a cleaning effect is achieved, and on the other hand, the surface of the material can be activated, which is conducive to the formation of alloys between the platinum and titanium in the intermediate layer and the lanthanum and platinum in the activation layer under high temperature conditions, thereby further enhancing the bonding strength between the substrate, the intermediate layer and the activation layer, and improving the stability of the active cathode.

[0021] In summary, the active cathode prepared by the preparation method provided by the present invention has a lower hydrogen evolution overpotential and a longer service life. It can be applied in the electrolytic chlorine production fields such as the chlor-alkali industry, chlorate production, and hypochlorite production to reduce energy consumption and use costs.

[0022] The present invention will be explained in detail below with reference to the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 1 is a polarization curve diagram of each embodiment and comparative example of the present invention; Figure 2 This is a surface SEM image of the active cathode prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings, but the present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.

[0025] Embodiment 1: An active cathode for electrolytic chlorine production, comprising a titanium mesh, an intermediate layer and an activation layer, is prepared as follows: S1. Matrix pretreatment: cut a 10*10 cm*1 mm titanium mesh, and sandblast it with 20-mesh brown corundum. The roughness of the titanium mesh after sandblasting is: Ra is 6-8 μm, Rz is 40-50 μm; then soak it in 10 wt% oxalic acid at 80 °C for 2 h, rinse it with pure water after soaking, and then dry it; S2. Preparation of the intermediate layer: Dissolve chloroplatinic acid in isopropanol with a platinum content of 0.4 g / L, then evenly coat it on the pretreated titanium mesh (coat both sides of the titanium mesh), sinter in a 500 °C sintering furnace for 30 min, repeat the coating and sintering three times after cooling, coating 0.15 mL each time, so that the thickness of the deposited intermediate layer is 210 nm; S3. Prepare the activation layer: dissolve ruthenium trichloride and lanthanum nitrate in hydrochloric acid and stir for 30 min, wherein the ratio of ruthenium to lanthanum is 4:1, then coat the solution on the intermediate layer and sinter in a 500 ℃ sintering furnace for 40 min. After cooling, repeat the coating and sintering for 5 times, coating 0.2 mL each time, so that the thickness of the deposited activation layer is 1 μm.

[0026] In the above steps S2 and S3, before the first coating, the titanium mesh is cleaned and activated in a plasma cleaning machine, and the cleaning and activation is carried out in an inert gas (such as nitrogen, argon, etc.) chamber, the discharge power is greater than 10 MHz, and the processing time is 5 minutes. This helps to form an alloy layer at the interface.

[0027] Embodiment 2: This embodiment differs from Embodiment 1 in that: In step S1, 16-mesh brown corundum is used for sandblasting, and the roughness of the titanium mesh after sandblasting is: Ra is 8-10 μm, and Rz is 50-60 μm; then it is immersed in 20 wt% hydrochloric acid at 80 ° C for 20 min, and then rinsed with pure water and dried.

[0028] The rest is the same as the first embodiment.

[0029] Embodiment 3: This embodiment differs from Embodiment 1 in that: In step S2, hydroxyplatinic acid is dissolved in isopropanol with a platinum content of 0.3 g / L, and then evenly coated on the pretreated titanium mesh and sintered in a 460°C sintering furnace for 30 min. After cooling, the coating and sintering are repeated 4 times, with 0.2 mL coated each time, so that the thickness of the deposited intermediate layer is 350 nm.

[0030] In steps S2 and S3 of this embodiment, before each coating, the titanium mesh is placed in a plasma cleaner for cleaning and activation. The cleaning and activation are performed in an inert gas (such as nitrogen, argon, etc.) chamber with a discharge power greater than 10 MHz and a processing time of 0.4 min.

[0031] The rest is the same as the first embodiment.

[0032] Embodiment 4: This embodiment differs from Embodiment 1 in that: In step S3, ruthenium trichloride and lanthanum carbonate are dissolved in a 1:1 isopropanol and n-butanol mixture and stirred for 30 min, wherein the ratio of ruthenium to lanthanum is 7:1, and then the solution is coated on the intermediate layer and sintered in a 520°C sintering furnace for 30 min. After cooling, the coating and sintering are repeated 8 times, with 0.25 mL coated each time, so that the thickness of the deposited activation layer is 2 μm.

[0033] Comparative Example 1: A steel wire mesh of 10*10 cm*1 mm low-carbon steel material is directly used as the cathode.

[0034] Comparative Example 2: A 10*10 cm*1 mm titanium mesh was directly used as the cathode.

[0035] Comparative Example 3: An active cathode, consisting of a titanium mesh and an activation layer, is prepared as follows: S1. Matrix pretreatment: cut a 10*10 cm*1 mm titanium mesh, and sandblast it with 20-mesh brown corundum. After sandblasting, the roughness Ra of the titanium mesh is 6-8 μm, and Rz is 40-50 μm. Then soak it in 10 wt% oxalic acid at 80 °C for 2 h, rinse it with pure water after soaking, and then dry it; S2. Prepare the activation layer: dissolve ruthenium trichloride in hydrochloric acid and stir for 30 min, then coat the solution on the pretreated titanium mesh and sinter in a 500 °C sintering furnace for 40 min. After cooling, repeat the coating and sintering for 5 times, coating 0.2 mL each time.

[0036] The cathodes prepared in the above-mentioned embodiments and comparative examples were subjected to accelerated aging life test and polarization curve test to obtain accelerated aging life and cathode polarization potential, and the specific contents are as follows: (1) Accelerated aging life test A DC power supply was used, the electrolyte was a saturated NaCl solution, and the water bath temperature was maintained at 60±1°C. The anode used a 1*1cm Ru-Ti-Ir ternary oxide anode, and the cathode used a 1*1cm cathode prepared in the embodiment and the comparative example, with a distance of 1 cm between the cathode and the anode. The constant current density was 500 A / m 2 In order to eliminate the interference of anode failure, a new Ru-Ti-Ir ternary oxide anode was replaced every 100 h of electrolysis. When the cell voltage rose sharply by 5 V, it was considered that the cathode failed. The test results are shown in Table 1.

[0037] (2) Polarization curve test In an electrochemical system, when electrode polarization occurs, the electrode potential of the anode always becomes more positive than the equilibrium potential, and the electrode potential of the cathode always becomes more negative than the equilibrium potential. Therefore, the negative movement of the electrode potential away from the equilibrium potential is called cathode polarization, and vice versa is anodic polarization. The cathode potential was tested using an electrochemical workstation using a constant current method in a three-electrode electrolytic cell. The reference electrode was a saturated calomel electrode, the auxiliary electrode was a platinum electrode, the working electrode was the cathode prepared in the examples and comparative examples, and the test area was 1 cm 2 , tested in saturated NaCl solution. The temperature was controlled at 25±0.5 ℃. The polarization curve was completed in the range of 0-1.5 V at a scan rate of 2 mV / s, and the cathode polarization potential was obtained from the polarization curve. The test results are shown in Table 1 and Figure 1 shown.

[0038] Table 1 Accelerated life test and polarization curve test data of the embodiments of the present invention and the comparative examples Classification Accelerated aging life (h) <![CDATA[Cathodic polarization potential (V) at a current density of 0.3 A / cm 2 > Example 1 1538 -1.18 Example 2 1572 -1.15 Example 3 1610 -1.12 Example 4 1564 -1.14 Comparative Example 1 980 -1.67 Comparative Example 2 1042 -1.72 Comparative Example 3 1347 -1.31 From Table 1 and Figure 1 It can be seen that by comparing the embodiment of the present invention with comparative examples 1 and 2, the life of the active cathode for electrolytic chlorine production prepared by the present invention is increased by about 1.5 times compared with the low-carbon steel or titanium commonly used in industry; at the same time, the hydrogen evolution performance of the active cathode is better than that of low-carbon steel or titanium cathode in the entire current density range. When the current density is 0.3A / cm 2 When the cathode hydrogen evolution overpotential is reduced by 490-600 mV, it is shown that the active cathode prepared by the present invention can significantly reduce the cell voltage when used as the cathode for electrolytic chlorine production.

[0039] From Table 1 and Figure 1 It can be seen that by comparing the embodiment of the present invention with Comparative Example 3, it can be seen that using platinum as the intermediate layer and introducing the rare earth element lanthanum into the activation layer can further increase the service life of the cathode and reduce the cathode hydrogen evolution overpotential.

[0040] The surface SEM image of the active cathode prepared in Example 1 of the present invention is as follows: Figure 2 As shown by Figure 2 It can be seen that the surface of the active cathode prepared in the present invention has many holes and cracks. This three-dimensional structure has a larger specific surface area, which increases the number of active sites exposed on the cathode surface and also plays a certain role in reducing the hydrogen evolution overpotential.

[0041] The above is an exemplary description of the present invention in combination with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as such non-substantial improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for preparing an active cathode for electrolytic chlorine production, characterized in that: The steps include: S1. Substrate pretreatment: using the titanium mesh as the substrate, sandblasting and etching it to form a rough surface of the titanium mesh; S2, preparing the intermediate layer: uniformly coating the platinum compound solution on the pretreated titanium mesh, and sintering at a high temperature to form the intermediate layer; S3. Preparation of an activation layer: coating a mixed solution of ruthenium trichloride and lanthanum compound on the intermediate layer, and forming an activation layer through high-temperature sintering.

2. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S1, after sandblasting, the surface roughness of the titanium mesh is: Ra is greater than 5 μm, and Rz is greater than 30 μm.

3. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S1, the etching is as follows: the titanium mesh is immersed in an inorganic acid solution at 80-110° C. for more than 10 minutes, and then rinsed with pure water and dried.

4. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S2, in the platinum compound solution, the platinum compound is at least one of chloroplatinic acid and hydroxyplatinic acid, the solvent used is an alcohol solution, and the content of platinum is 0.1-0.5 g / L.

5. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S2, the high temperature sintering temperature is 400-600°C, the sintering time is greater than 20 min, and the coating and sintering are repeated 2-5 times to make the thickness of the deposited intermediate layer 100-500 nm.

6. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S3, in the mixed solution of ruthenium trichloride and lanthanum compound, the lanthanum compound is at least one of lanthanum nitrate and lanthanum carbonate, the solvent used is hydrochloric acid or alcohol solution, and the ratio of ruthenium to lanthanum is 3:1-10:

1.

7. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In step S3, the high temperature sintering temperature is 420-550°C, the sintering time is greater than 30 min, and the coating sintering is repeated 4-10 times to make the thickness of the deposited activation layer 0.5-3 μm.

8. The method for preparing an active cathode for electrolytic chlorine production according to claim 1, characterized in that: In steps S2 and S3, before the first coating, the titanium mesh is placed in a plasma cleaner for cleaning and activation.

9. The method for preparing an active cathode for electrolytic chlorine production according to claim 8, characterized in that: The cleaning and activation is carried out in an inert gas chamber, the discharge power is greater than 10 MHz, and the processing time is 0.4-5 min.

10. An active cathode for electrolytic chlorine production, characterized in that: The active cathode comprises a titanium mesh and an intermediate layer and an activation layer attached to the titanium mesh; the active cathode is prepared by the preparation method according to any one of claims 1 to 9.