Polyimide fiber as well as preparation method and application thereof

By introducing amino-modified polysilsesquioxane and diamine monomer into the polyimide fiber, a copolymerized polyimide fiber is formed, and a passivation layer is formed using phosphorus and silicon-containing structural units to form, which solves the polyamide The problem of atomic oxygen erosion in low-Earth orbit environments has significantly improved the atomic oxygen resistance of fibers.

CN119041048APending Publication Date: 2024-11-29CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411386060.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Polyimide materials are deteriorated by atomic oxygen erosion in low-Earth orbit space environments, and need to be modified to obtain excellent atomic oxygen resistance.

Method used

The amino-modified polysilsesquioxane, dianhydride monomer and diamine monomer are used for spinning and imidation treatment, phosphorus-containing and silicon-containing structural units are introduced to form copolymerized polyimide fibers, and through hydrogen bonds and nanoparticles enriched to form a passivation layer to prevent atomic oxygen erosion.

Benefits of technology

The atomic oxygen resistance of polyimide fibers is improved, the aggregation of spinning liquid is avoided, the strength and modulus of the fiber are enhanced, and atomic oxygen erosion is effectively prevented by forming a passivation layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_15
    Figure SMS_15
  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The invention provides a polyimide fiber as well as a preparation method and application thereof. The polyimide fiber is obtained by carrying out spinning and imidization treatment on reactants of amino-modified polysilsesquioxane, a dianhydride monomer and a diamine monomer. According to the invention, a phosphorus-containing structural unit (i.e., a first diamine monomer) is introduced into a polyimide molecular chain through a copolymerization reaction. Besides, amino-modified polysilsesquioxane, a diamine monomer and a dianhydride monomer are subjected to in-situ copolymerization, the dispersity of the polysilsesquioxane in a spinning solution is improved, meanwhile, a silicon-containing structural unit is introduced into a polyimide molecular chain, and through the synergistic effect of phosphorus and silicon, the polysilsesquioxane / polyimide composite material is prepared. The prepared polyimide fiber material has excellent atomic oxygen resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polyimide fiber and a preparation method and application thereof. Background Art

[0002] Low Earth orbit usually refers to an orbit 200 to 1000 km from the Earth's surface. The spacecraft in service in this orbit mainly include space stations, reconnaissance satellites, meteorological satellites or spacecraft. The space environment of low Earth orbit mainly includes hot and cold cycles, space debris, high-energy particles, ultraviolet radiation and atomic oxygen radiation. Studies have shown that atomic oxygen is one of the most serious orbital space environments for spacecraft surface corrosion. The main reason is that atomic oxygen is highly oxidizing and the collision energy between atomic oxygen and the spacecraft surface can reach 4 to 5 eV. When atomic oxygen interacts with the surface of the spacecraft, it will break the chemical bonds of the spacecraft surface material, causing erosion and performance degradation.

[0003] Polyimide materials are widely used in spacecraft due to their excellent properties such as high strength and modulus, radiation resistance, good dimensional stability, high and low temperature resistance, low vacuum mass loss and vacuum condensable volatiles, and solvent resistance. However, polyimide materials will degrade in performance after being corroded by atomic oxygen. Therefore, it is necessary to modify them to obtain polyimide materials with excellent atomic oxygen resistance. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a polyimide fiber and a preparation method and application thereof. The polyimide fiber has excellent atomic oxygen resistance.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a polyimide fiber, which is obtained by spinning and imidization of reactants of amino-modified polysilsesquioxane, dianhydride monomer, and diamine monomer;

[0007] The structural formula of the amino-modified polysilsesquioxane is shown in Formula I:

[0008] Formula I;

[0009] Among them, R1 is or ; n is any integer from 1 to 6; R2 is N((CH2) x (CH3) y ) z , X is any integer between 0 and 6, y is 1, and z is 2 or 3;

[0010] The diamine monomer includes a first diamine monomer and a second diamine monomer;

[0011] The first diamine monomer is an aromatic diamine monomer containing P=O.

[0012] Preferably, the content of the amino-modified polysilsesquioxane is 5-45 wt % of the sum of the mass of the dianhydride monomer and the diamine monomer.

[0013] Preferably, the molar ratio of the dianhydride monomer to the diamine monomer is 1:(0.9-1.3).

[0014] Preferably, the molar ratio of the first diamine monomer to the second diamine monomer is (0.1-0.5):(0.5-0.9).

[0015] Preferably, the amino-modified polysilsesquioxane is selected from any one or more of the following formulas Ⅰ-1 to Ⅰ-6:

[0016] .

[0017] Preferably, the dianhydride monomer is selected from any one or more of formulas (1) to (11):

[0018] .

[0019] Preferably, the first diamine monomer is selected from any one or more of the following formulas (II-1) to (II-11):

[0020] .

[0021] Preferably, the second diamine monomer is selected from any one or more of the following formulas (ⅠⅡ-1) to (ⅠⅡ-16):

[0022] .

[0023] In a second aspect, the present invention provides a method for preparing the above-mentioned polyimide fiber, comprising the following steps:

[0024] The amino-modified polysilsesquioxane shown in formula I, the first diamine monomer, the second diamine monomer, and the dianhydride monomer are mixed and reacted, and spun to obtain polyamic acid fibers;

[0025] The polyamic acid fiber is imidized to obtain polyimide fiber.

[0026] Preferably, the imidization treatment further includes a heat stretching step, and the heat stretching is performed in an inert atmosphere.

[0027] Preferably, the temperature of the heat drawing is 350-600°C.

[0028] Preferably, the thermal stretching ratio is 1.0 to 5.0 times.

[0029] Preferably, the imidization treatment adopts gradient temperature rising heat treatment or constant temperature heat treatment, and the imidization treatment is carried out in vacuum or inert atmosphere.

[0030] Preferably, the temperature of the gradient temperature increase heat treatment is 50-520° C., and the heating rate is 1-30° C. / min.

[0031] Preferably, the isothermal heat treatment is performed at a temperature of 300-520° C. and for a time of 5-60 min.

[0032] In a third aspect, the present invention provides an application of the polyimide fiber involved in the above technical solution in the aerospace field.

[0033] In a fourth aspect, the present invention provides an application of a low earth orbit space vehicle, which includes the polyimide fiber involved in the above technical solution.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a polyimide fiber, which is obtained by spinning and imidizing a mixture of amino-modified polysilsesquioxane, dianhydride monomer, and diamine monomer. In the present invention, a phosphorus-containing structural unit (i.e., a first diamine monomer) is introduced into a polyimide molecular chain through a copolymerization reaction. In addition, the present invention in situ copolymerizes the amino-modified polysilsesquioxane with a diamine monomer and a dianhydride monomer to increase the dispersibility of the polysilsesquioxane in the spinning solution while introducing a silicon-containing structural unit into the polyimide molecular chain. When the amino group introduced into the amino-modified polysilsesquioxane is a tertiary amine, it can form a hydrogen bond interaction with polyamic acid, so that the polysilsesquioxane can be more evenly dispersed in the polyamic acid spinning solution. On the one hand, the aggregation of the polysilsesquioxane in the polyamic acid spinning solution is avoided, so that the spinnability of the spinning solution is not affected. On the other hand, the obtained polyimide composite fiber has no obvious defects and no stress concentration points, thereby improving the strength and modulus of the fiber. When the amino group introduced into the amino-modified polysilsesquioxane is a quaternary ammonium salt, the dipole moment of the obtained nanoparticles is large. When the spinning solution filaments are double-diffusion spun through the coagulation bath, a large number of nanoparticles will diffuse to the fiber surface with the polar solvent to form enrichment. For the polyimide fiber system containing tertiary amine-modified polysilsesquioxane, when atomic oxygen is irradiated to the surface of the polyimide fiber, P=O and P-Ar are destroyed to form phosphate (ester), and Si atoms exist in the form of SiO2. The passivation layer formed by the two synergistically prevents the atomic oxygen from further corroding the fiber. For the polyimide fiber system containing quaternary ammonium salt-modified polysilsesquioxane, when atomic oxygen is irradiated to the surface of the polyimide fiber, the Si element enriched on the fiber surface exists in the form of SiO2, and the P element distributed inside the fiber exists in the form of phosphate (ester), forming a gradient atomic oxygen resistance effect, thereby giving the polyimide fiber excellent atomic oxygen resistance. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The present invention provides a polyimide fiber, which is obtained by spinning and imidization of reactants of amino-modified polysilsesquioxane, dianhydride monomer, and diamine monomer. The content of the amino-modified polysilsesquioxane is 5-45 wt% of the sum of the mass of the dianhydride monomer and the diamine monomer, preferably 10-40 wt%, and more preferably 15-30 wt%; the molar ratio of the dianhydride monomer to the diamine monomer is 1:(0.9-1.3), preferably 1:(1.0-1.2).

[0038] In the present invention, the structural formula of the amino-modified polysilsesquioxane is as shown in Formula I:

[0039] Formula I ;

[0040] Among them, R1 is or ; n is any integer from 1 to 6, which can be selected from 1, 2, 3, 4, 5 or 6; R2 is N((CH2) x (CH3) y ) z , X is any integer between 0 and 6, which can be selected from 1, 2, 3, 4, 5 or 6; y is 1; and z is 2 or 3.

[0041] The present invention adopts amino-modified polysilsesquioxane. Compared with unmodified polysilsesquioxane, when the amino group introduced into the amino-modified polysilsesquioxane is a tertiary amine, it can form hydrogen bond interaction with polyamic acid, so that the polysilsesquioxane can be more evenly dispersed in the polyamic acid spinning solution. On the one hand, the aggregation of the polysilsesquioxane in the spinning solution is avoided, so that the spinnability of the spinning solution is not affected. On the other hand, the obtained polyimide composite fiber has no obvious defects and no stress concentration points, thereby improving the strength and modulus of the fiber. When the amino group introduced into the amino-modified polysilsesquioxane is a quaternary ammonium salt, the dipole moment of the nanoparticles obtained at this time is large. When the spinning solution filaments are subjected to double diffusion spinning through a coagulation bath, the nanoparticles will diffuse to the fiber surface following the polar solvent. For the polyimide fiber system containing tertiary amine modified polysilsesquioxane, when atomic oxygen is irradiated to the surface of the polyimide fiber, P=O and P-Ar are destroyed to form phosphate (ester), and Si atoms exist in the form of SiO2. The passivation layer formed by the two synergistically prevents the atomic oxygen from further corroding the fiber. For the polyimide fiber system containing quaternary ammonium salt modified polysilsesquioxane, when atomic oxygen is irradiated to the surface of the polyimide fiber, the Si element enriched on the fiber surface exists in the form of SiO2, and the P element distributed inside the fiber exists in the form of phosphate (ester), forming a gradient atomic oxygen resistance effect, thereby giving the polyimide fiber excellent atomic oxygen resistance.

[0042] In some embodiments of the present invention, the amino-modified polysilsesquioxane is selected from any one or more of the following formulas Ⅰ-1 to Ⅰ-6:

[0043] .

[0044] It can be seen that in the present invention, the amino-modified polysilsesquioxane includes polysilsesquioxane modified with tertiary amine and quaternary ammonium salt.

[0045] In the present invention, the diamine monomer includes a first diamine monomer and a second diamine monomer; the first diamine monomer is an aromatic diamine monomer containing P=O, specifically selected from any one or more of the following formulas (II-1) to (II-11):

[0046] .

[0047] In the present invention, the second diamine monomer is a commercially available diamine monomer or a heterocyclic diamine monomer.

[0048] In some embodiments of the present invention, the second diamine monomer is selected from any one or more of the following formulas (III-1) to (III-16):

[0049] .

[0050] The present invention adopts the first diamine monomer and the second diamine monomer as diamine monomers, because after only the first diamine monomer as the source of the phosphorus-containing structural unit is introduced, the polymerization activity of the monomer is low, and a high molecular weight polymer spinning solution cannot be obtained, and thus a polyimide fiber with good comprehensive performance or even good molding performance cannot be obtained. The second diamine monomer has a high polymerization activity, and adding it to the polymerization system of the first diamine monomer and the dianhydride monomer can adjust the molecular weight of the polymer spinning solution, so that the molecular weight and viscosity of the spinning solution reach the range of spinnability; in addition, some preferred second diamine monomers are introduced, and intramolecular and intermolecular hydrogen bonds can be formed in the polyimide system, thereby improving the comprehensive performance of the fiber. In some embodiments of the present invention, the molar ratio of the first diamine monomer to the second diamine monomer is (0.1~0.5): (0.5~0.9), preferably (0.2~0.4): (0.6~0.8).

[0051] In the present invention, the dianhydride monomer is one of the main monomers for synthesizing polyimide, and can be selected from any one or more of formulas (1) to (11):

[0052] .

[0053] The present invention also provides a method for preparing the polyimide fiber, comprising the following steps:

[0054] The amino-modified polysilsesquioxane of formula I, the first diamine monomer of formula II, the second diamine monomer of formula III, and the dianhydride monomer are mixed and reacted, and spun to obtain polyamic acid fibers;

[0055] The polyamic acid fiber is imidized to obtain polyimide fiber.

[0056] In the invention, the amino-modified polysilsesquioxane shown in formula I, the first diamine monomer, the second diamine monomer, and the dianhydride monomer are mixed and reacted in proportion to obtain a polyamic acid spinning solution, and the concentration of the polyamic acid spinning solution is 5~40 wt%, preferably 10~30 wt%. The present invention controls the above concentration range in order to control the molecular weight and viscosity of the spinning solution so that the spinning solution has good spinnability. In some embodiments of the present invention, the reaction is a polymerization reaction, preferably occurring in a polar aprotic solvent, and the polar aprotic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or N-methylpyrrolidone. Wherein, the temperature of the polymerization reaction is -20~55°C, preferably -10~40°C; the time is 4~60 h, preferably 10~50 h.

[0057] In some embodiments of the present invention, the obtained polyamic acid spinning stock solution is preferably first filtered and vacuum degassed to obtain a spinning solution, and then spun using a spinning molding process to obtain polyamic acid fibers.

[0058] The present invention has no particular limitation on the methods of filtration and vacuum degassing, and any filtration and vacuum degassing methods known to those skilled in the art may be used.

[0059] Likewise, the present invention has no particular limitation on the spinning method, which may be any one of wet spinning, dry spinning or dry-jet-wet spinning, preferably wet spinning or dry-jet-wet spinning.

[0060] Exemplarily, the dry-wet spinning process can be carried out as follows: the obtained spinning solution is extruded from the spinneret through a metering pump, passes through an air layer and enters a coagulation bath for forming, and then is drawn and washed, and dried by a hot roller or a tunnel to obtain the polyamic acid fiber. The coagulation bath used is preferably a mixture of any one of ethanol, ethylene glycol, butanol, acetone and butanone with water, or a mixture of any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone with water; the drying environment is preferably air, nitrogen, argon or other inert gases; the height of the air layer is preferably 3-80 mm, more preferably 10-50 mm; the aperture of the spinneret is preferably Φ0.03-Φ0.3 mm, more preferably Φ0.05-Φ0.2 mm; the number of holes is preferably 20-4000 holes, preferably 100-3000 holes; the spray-to-pulling ratio is preferably 1.5-7.0 times, more preferably 2.0-5.0 times; the speed is preferably 10-100 m / min, more preferably 20-80 m / min.

[0061] Exemplarily, the wet spinning process can be carried out as follows: the obtained spinning solution is extruded from the spinneret through a metering pump, directly enters the coagulation bath for forming, and then is drawn, washed, and dried by a hot roller or hot tunnel to obtain polyamic acid fiber. The coagulation bath used is preferably a mixture of any one of ethanol, ethylene glycol, butanol, acetone and butanone with water, or a mixture of any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone with water; the drying environment is preferably air, nitrogen, argon or other inert gases; the aperture of the spinneret is preferably Φ0.04~Φ0.15mm, more preferably Φ0.05~Φ0.10 mm; the number of holes is preferably 30~8000 holes, more preferably 100~6000 holes; the spray-pull ratio is preferably 1.1~6.0 times, more preferably 2.0~4.0 times; the speed is 5~80 m / min, more preferably 10~70 m / min.

[0062] Exemplarily, the dry spinning process is carried out as follows: the obtained spinning solution is extruded from the spinneret hole by a metering pump, directly passes through a long hot tunnel, removes the solvent and is formed, and at the same time, under the action of winding tension, it is stretched and thinned to obtain polyamic acid fiber.

[0063] After spinning is completed and polyamic acid fibers are obtained, according to the present invention, the polyamic acid fibers are preferably subjected to imidization treatment to obtain polyimide fibers. In the present invention, the imidization treatment is carried out in a vacuum or inert atmosphere, preferably a nitrogen or argon atmosphere.

[0064] In the present invention, the imidization treatment adopts gradient temperature rise heat treatment or constant temperature heat treatment, wherein the temperature of the gradient temperature rise heat treatment is 50~520℃, that is, the temperature rises from 50℃ to 520℃, preferably 50~450℃; the heating rate is 1~30℃ / min, preferably 5~20℃ / min, and more preferably 10~15℃ / min.

[0065] The isothermal heat treatment is performed at a temperature of 300-520° C., preferably 350-450° C., and for a time of 5-60 min, preferably 10-40 min.

[0066] In some embodiments of the present invention, a heat stretching step is further included after the imidization treatment to improve the performance of the polyimide fiber. The heat stretching is performed in an inert atmosphere, preferably a nitrogen or argon atmosphere; the heat stretching temperature is 350-600°C, preferably 400-500°C; the heat stretching ratio is 1.0-5.0 times, preferably 1.5-3.0 times.

[0067] The preparation method of the polyimide fiber provided by the present invention has simple process, high process controllability, and is easy to industrialize, and is applicable to various spinning molding methods.

[0068] The polyimide fiber prepared by the present invention contains silicon and phosphorus structural units at the same time, so the fiber has excellent atomic oxygen resistance, which improves the atomic oxygen resistance of existing polyimide fibers. Based on this, the present invention also provides an application of the above-mentioned polyimide fiber in the aerospace field.

[0069] In particular, the present invention also provides an application of a low earth orbit spacecraft, which includes the polyimide fiber involved in the above technical solution.

[0070] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products.

[0071] Example 1

[0072] 160.19 g (0.80 mol) of III-5, 75.26 g (0.20 mol) of II-3 and 52.97 g of I-4 were dissolved in 4200 mL of N,N'-dimethylacetamide, and 294.22 g (1.00 mol) of dianhydride monomer (7) was added under stirring at 20°C, and the mixture was polymerized at 20°C for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0073] The spinning slurry is spun into shape by dry-jet wet spinning technology. The spinning slurry at room temperature is accurately metered by a metering pump, extruded from the spinneret, passed through the air layer and entered into a coagulation bath of N,N'-dimethylacetamide and water with a volume ratio of 1:8, and then drawn, washed with water, and dried in a hot argon channel to obtain polyamic acid fiber. The spinneret has 100 holes, a hole diameter of Φ0.15 mm, a spray-draw ratio of 4.0 times, a spinning speed of 80 m / min, and an air layer height of 15 mm.

[0074] The polyamic acid fiber is subjected to a thermal imidization treatment by gradient heating in a vacuum environment to obtain a polyimide fiber. The thermal imidization temperature is increased from 50°C to 400°C at a heating rate of 15°C / min;

[0075] The obtained polyimide fiber was stretched 3.0 times at 450° C. in an argon environment to obtain a polyimide finished fiber.

[0076] Example 2

[0077] 75.70 g (0.70 mol) of III-2, 112.90 g (0.30 mol) of II-4, and 110.18 g of I-5 were dissolved in 4400 mL of N,N'-dimethylformamide, and 161.12 g (0.50 mol) of dianhydride monomer (4) and 201.16 g (0.50 mol) of dianhydride monomer (9) were added under stirring at 10°C, and the mixture was polymerized at 15°C for 20 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0078] The spinning slurry is spun into shape by wet spinning technology. The spinning slurry at room temperature is accurately metered by a metering pump, extruded from the spinneret hole and directly enters into a coagulation bath of ethanol and water with a volume ratio of 2:7, and then drawn, washed, and dried in a hot air channel to obtain polyamic acid fiber. The spinneret has 500 holes, a hole diameter of Φ0.05 mm, a spray-draw ratio of 2.0 times, and a speed of 30 m / min.

[0079] The polyamic acid fiber was treated in a gradient heating thermal imidization furnace under an argon environment to obtain polyimide fiber. The thermal imidization temperature was increased from 50°C to 410°C at a heating rate of 20°C / min.

[0080] The obtained polyimide fiber was stretched 2.0 times at 460° C. in an argon environment to obtain a polyimide finished fiber.

[0081] Example 3

[0082] 64.88 g (0.60 mol) of III-2, 67.28 g (0.30 mol) of III-10 and 62.85 g (0.10 mol) of (II-11) and 123.94 g of I-1 were dissolved in 4470 mL of N-methylpyrrolidone, and 218.12 g (1.00 mol) of dianhydride monomer (1) was added under stirring, and the mixture was polymerized at 10° C. for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0083] The spinning slurry is spun into shape by dry-jet wet spinning technology. The spinning slurry at room temperature is accurately metered by a metering pump, extruded from the spinneret hole, and then passed through an air layer into a coagulation bath of N-methylpyrrolidone and water with a volume ratio of 1:5, and then drawn, washed, and dried in a hot nitrogen channel to obtain polyamic acid fiber. The spinneret has 500 holes, a hole diameter of Φ0.12 mm, a spray-to-draw ratio of 3.5 times, a spinning speed of 70 m / min, and an air layer height of 20 mm.

[0084] The polyamic acid fiber was treated in a gradient heating thermal imidization furnace under nitrogen environment to obtain polyimide fiber. The thermal imidization temperature was increased from 50°C to 430°C at a heating rate of 15°C / min.

[0085] The obtained polyimide fiber was stretched 1.5 times at 470° C. in a nitrogen environment to obtain a polyimide finished fiber.

[0086] Example 4

[0087] 157.68 g (0.70 mol) III-11, 46.25 g (0.15 mol) II-2, 66.65 g (0.15 mol) II-8, 15.10 g I-3 and 15.10 g I-6 were dissolved in 3860 mL N,N'-dimethylacetamide, 174.50 g (0.800 mol) dianhydride monomer (1) and 104.10 g (0.200 mol) dianhydride monomer (10) were added under stirring at -10°C, and the polymerization was maintained at -10°C for 12 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing.

[0088] The spinning slurry is spun into shape by dry-jet wet spinning. The spinning slurry at room temperature is accurately metered by a metering pump, extruded from the spinneret, passed through the air layer and entered into a coagulation bath of N,N'-dimethylacetamide and water with a volume ratio of 1:3.5, and then drawn, washed with water, and dried in a hot nitrogen channel to obtain polyamic acid fiber. The spinneret has 500 holes, a hole diameter of Φ0.20 mm, a spray-to-draw ratio of 4.0 times, a spinning speed of 70 m / min, and an air layer height of 13 mm.

[0089] The polyamic acid fiber was treated in a gradient heating thermal imidization furnace under a hot nitrogen environment to obtain polyimide fiber. The thermal imidization temperature was increased from 50°C to 450°C at a heating rate of 10°C / min.

[0090] The obtained polyimide fiber was stretched 2.0 times at 480° C. in a nitrogen environment to obtain a polyimide finished fiber.

[0091] Example 5

[0092] 43.26 g (0.40 mol) of III-1, 104.93 g (0.40 mol) of III-14, 125.63 g (0.200 mol) of II-5 and 81.60 g of I-2 were dissolved in 3100 mL of dimethyl sulfoxide, 174.50 g (0.80 mol) of dianhydride monomer (1) and 95.68 g (0.20 mol) of dianhydride monomer (11) were added under stirring at -15°C, and the mixture was polymerized for 12 h at -15°C to obtain a viscous polyamic acid spinning solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0093] The spinning slurry is formed by dry-jet wet spinning, and the spinning slurry at room temperature is accurately measured by a metering pump, extruded from the spinneret, passed through the air layer and entered into a coagulation bath of dimethyl sulfoxide and water with a volume ratio of 1:5, and then drawn, washed, and dried in a hot nitrogen channel to obtain polyamic acid fiber. The spinneret has 200 holes, the hole diameter is Φ0.18 mm, the spray-to-draw ratio is 2.0 times, the spinning speed is 60 m / min, and the air layer height is 15 mm;

[0094] The polyamic acid fiber was treated in a gradient temperature-increasing thermal imidization furnace under a nitrogen environment to obtain polyimide fiber. The thermal imidization temperature was increased from 50°C to 460°C at a rate of 5°C / min.

[0095] The obtained polyimide fiber was stretched 3.0 times at 490° C. in a nitrogen environment to obtain a polyimide finished fiber.

[0096] Example 6

[0097] 54.07 g (0.50 mol) of III-2, 112.14 g (0.500 mol) of III-10, 24.63 g (0.05 mol) of II-6, 17.02 g (0.05 mol) of II-10 and 85.20 g of I-6 were dissolved in 3000 mL of N-methylpyrrolidone, 218.12 g (1.00 mol) of dianhydride monomer (1) was added under stirring, and the mixture was polymerized at -10°C for 12 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0098] The spinning slurry is spun into shape by using the dry-jet wet spinning technology. The spinning slurry at room temperature is accurately metered by a metering pump, extruded from the spinneret hole, and then passed through the air layer into a coagulation bath of N-methylpyrrolidone and water with a volume ratio of 1:4, and then drawn, washed, and dried in a hot nitrogen channel to obtain polyamic acid fibers. The spinneret has 1000 holes, a hole diameter of Φ0.12 mm, a spray-draw ratio of 3.0 times, a spinning speed of 90 m / min, and an air layer height of 20 mm.

[0099] The polyamic acid fiber was treated in a gradient heating thermal imidization furnace under nitrogen environment to obtain polyimide fiber. The thermal imidization temperature ranged from 50 to 450°C, and the heating rate was 10°C / min.

[0100] The obtained polyimide fiber was stretched 2.5 times at 490° C. in a nitrogen environment to obtain a polyimide finished fiber.

[0101] Comparative Example 1

[0102] 200.24 g (1.00 mol) of III-5 was dissolved in 4200 mL of N,N'-dimethylacetamide, and 294.22 g (1.00 mol) of dianhydride monomer (7) was added under stirring at 20°C, and the mixture was polymerized at 20°C for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0103] The spinning slurry is spun into shape by the same spinning process as in Example 1 to obtain polyamic acid fibers, which are then treated by the same imidization process as in Example 1 to obtain polyimide fibers, and finally heat-stretched by the same process as in Example 1 to obtain polyimide finished fibers.

[0104] Comparative Example 2

[0105] 64.88 g (0.60 mol) of III-2 and 67.28 g (0.30 mol) of III-10 were dissolved in 4470 mL of N-methylpyrrolidone, and 196.31 g (0.90 mol) of dianhydride monomer (1) was added under stirring, and the mixture was polymerized at 10° C. for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0106] The spinning slurry is spun into shape by the same spinning process as in Example 3 to obtain polyamic acid fibers, which are then treated by the same imidization process as in Example 3 to obtain polyimide fibers, and finally heat-stretched by the same process as in Example 3 to obtain polyimide finished fibers.

[0107] Comparative Example 3

[0108] 160.19 g (0.80 mol) of III-5 and 75.26 g (0.20 mol) of II-3 were dissolved in 4200 mL of N,N'-dimethylacetamide, and 294.22 g (1.00 mol) of dianhydride monomer (7) was added under stirring at 20°C, and the mixture was polymerized at 20°C for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing;

[0109] The spinning slurry is spun into shape by the same spinning process as in Example 1 to obtain polyamic acid fibers, which are then treated by the same imidization process as in Example 1 to obtain polyimide fibers, and finally heat-stretched by the same process as in Example 1 to obtain polyimide finished fibers.

[0110] Comparative Example 4

[0111] 200.24 g (1.00 mol) of III-5 and 52.97 g of I-4 were dissolved in 4200 mL of N,N'-dimethylacetamide, and 294.22 g (1.00 mol) of dianhydride monomer (7) was added under stirring at 20°C. The polymerization was maintained at 20°C for 10 h to obtain a viscous polyamic acid solution, which was used as a spinning slurry after filtration and vacuum degassing.

[0112] The spinning slurry is spun into shape by the same spinning process as in Example 1 to obtain polyamic acid fibers, which are then treated by the same imidization process as in Example 1 to obtain polyimide fibers, and finally heat-stretched by the same process as in Example 1 to obtain polyimide finished fibers.

[0113] The obtained polyimide fiber was tested for its atomic oxygen resistance. The fiber was mainly tested by 7×10 20 atoms·cm -2 The breaking strength changes before and after atomic oxygen erosion, the test results are shown in Table 1 below (the breaking strength test standard of the fiber is GB / T 14344-2008 Test method for tensile properties of chemical fiber filaments).

[0114] Table 1. Atomic oxygen irradiation resistance of polyimide fibers

[0115]

[0116] It can be seen from the data in Table 1 that the polyimide fiber prepared in the embodiment of the present invention has significant atomic oxygen resistance. By comparing Example 1 with Comparative Example 1, it can be seen that the polyimide fiber without Si and P elements in the system has poor atomic oxygen resistance, 7×10 20 atoms·cm -2The retention rate of the breaking strength of the polyimide fiber after atomic oxygen erosion is 48.2%. By comparing Example 3 with Comparative Example 2, it can be seen that the atomic oxygen resistance of the polyimide fiber without Si and P elements in the system is poor, 7×10 20 atoms·cm -2 The retention rate of the breaking strength of the polyimide fiber after atomic oxygen erosion is 45.1%. By comparing Example 1 with Comparative Example 3, it can be seen that the polyimide fiber without Si element in the system is 7×10 20 atoms·cm -2 After atomic oxygen erosion, the breaking strength retention rate of the polyimide fiber is 70.7%. By comparing Example 1 with Comparative Example 4, it can be seen that the polyimide fiber without P element in the system is eroded by 7×10 20 atoms·cm -2 After atomic oxygen corrosion, the breaking strength retention rate of polyimide fiber is 79.4%.

[0117] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A polyimide fiber, characterized in that: The product of amino-modified polysilsesquioxane, dianhydride monomer and diamine monomer is spun and imidized to obtain the product; The structural formula of the amino-modified polysilsesquioxane is shown in Formula I: Formula I; Among them, R1 is or ; n is any integer from 1 to 6; R2 is N((CH2) x (CH3) y ) z , X is any integer between 0 and 6, y is 1, and z is 2 or 3; The diamine monomer includes a first diamine monomer and a second diamine monomer; The first diamine monomer is an aromatic diamine monomer containing P=O.

2. The polyimide fiber according to claim 1, characterized in that: The content of the amino-modified polysilsesquioxane is 5-45 wt% of the sum of the mass of the dianhydride monomer and the diamine monomer; The molar ratio of the dianhydride monomer to the diamine monomer is 1:(0.9-1.3); The molar ratio of the first diamine monomer to the second diamine monomer is (0.1-0.5):(0.5-0.9).

3. The polyimide fiber according to claim 1 or 2, characterized in that: The amino-modified polysilsesquioxane is selected from any one or more of the following formulas Ⅰ-1 to Ⅰ-6: 。 4. The polyimide fiber according to any one of claims 1 to 3, characterized in that The dianhydride monomer is selected from any one or more of formulas (1) to (11): 。 5. The polyimide fiber according to any one of claims 1 to 4, characterized in that The first diamine monomer is selected from any one or more of the following formulas (II-1) to (II-11): ; The second diamine monomer is selected from any one or more of the following formulas (ⅠⅡ-1) to (ⅠⅡ-16): 。 6. A method for preparing a polyimide fiber as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: The amino-modified polysilsesquioxane shown in formula I, the first diamine monomer, the second diamine monomer, and the dianhydride monomer are mixed and reacted, and spun to obtain polyamic acid fibers; The polyamic acid fiber is imidized to obtain polyimide fiber.

7. The preparation method according to claim 6, characterized in that: The method further comprises a heat stretching step after the imidization treatment, wherein the heat stretching is performed in an inert atmosphere; The temperature of the heat drawing is 350-600°C; The thermal stretching ratio is 1.0 to 5.0 times.

8. The preparation method according to claim 6 or 7, characterized in that: The imidization treatment adopts gradient temperature rising heat treatment or constant temperature heat treatment, and the imidization treatment is carried out in vacuum or inert atmosphere; The temperature of the gradient heating heat treatment is 50-520°C, and the heating rate is 1-30°C / min; The temperature of the isothermal heat treatment is 300-520° C. and the time is 5-60 min.

9. Use of the polyimide fiber according to any one of claims 1 to 5 or the polyimide fiber prepared by the preparation method according to any one of claims 6 to 9 in the field of aerospace.

10. A spacecraft for use in a low earth orbit, characterized in that: The invention comprises the polyimide fiber according to any one of claims 1 to 5 or the polyimide fiber prepared by the preparation method according to any one of claims 6 to 9.

Citation Information

Cited By

  • Preparation process of antibacterial modified silicone rubber composite material

    CN119875377A

  • Preparation method of stretchable transparent electrode with spiral conductive nanofiber and electrode thereof

    CN120748850A

  • A method for preparing a stretchable transparent electrode having helical conductive nanofibers and an electrode thereof

    CN120748850B