Nanofiber preservative film as well as preparation method and application thereof
By spraying palm wax and silica on the starch nanofiber membrane, combined with octenyl succinate-tanninic acid-selenium nanoparticles, the problem of hydrophobicity and functional inadequate of starch nanofiber membrane was solved, and the problem of insufficient hydrophobicity and functionality of the starch nanofiber membrane was achieved. Effective preservation of fruits and reuse of selenium nanoparticles.
Patent Information
- Application Number
- CN202411235654.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
The existing starch nanofiber plastic wrap has poor hydrophobicity and is not rich in functionality, making it difficult to effectively prevent fruit rot, and the selenium nanoparticles have poor stability, which affects its biological activity and utilization.
The nanofiber membrane was prepared by electrospinyl succinate starch ester-tanninic acid-selenium nanoparticles and plulandosaccharides, and the membrane was sprayed with palma wax and silica to form a superhydrophobic layer. Enhance barrier properties, mechanical properties and oxidation resistance.
The prepared nanofiber plastic wrap is superhydrophobic, which can effectively prevent fruit from rotting, extend shelf life, and degrade in water, realize the reuse of selenium nanoparticles and improve the food preservation effect.
Smart Images

Figure CN119041200A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of daily necessities, and in particular to a nanofiber cling film and a preparation method and application thereof. Background Art
[0002] Fruits have ideal flavors and are rich in nutrients such as polyphenols and vitamins, and are favored by consumers. However, most fruits are sensitive and easily damaged, and are prone to oxidation and microbial attack. Traditional petroleum-based plastics are widely used in the field of food cling film, but they are difficult to degrade and will cause environmental pollution. Therefore, it is extremely necessary to develop a biodegradable and environmentally friendly food cling film. Starch is a common high-molecular carbohydrate in nature, with the advantages of wide sources, short regeneration cycle, low price, safety and non-toxicity, and easy processing. However, starch nanofiber cling film rich in hydroxyl groups has disadvantages such as hydrophilicity and lack of functionality, which limits its practical application to a certain extent.
[0003] Selenium nanoparticles have the advantages of high bioavailability, bioactivity and biosafety, and have been widely used in the field of antimicrobial agents. However, naked selenium nanoparticles are very unstable. Not only are their morphology and size difficult to control, but they also tend to spontaneously aggregate into gray or black selenium, which leads to a sharp drop in bioactivity and bioavailability, and a loss of efficacy. Summary of the invention
[0004] The main purpose of the present invention is to provide a nanofiber cling film and a preparation method and application thereof, aiming to solve the problems of poor hydrophobicity and limited functionality of the existing starch nanofiber cling film.
[0005] To achieve the above object, the present invention provides a method for preparing a nanofiber cling film, comprising the following steps:
[0006] S10. Providing octenyl succinate starch ester - tannic acid - selenium nanoparticles, mixing octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester - tannic acid - selenium nanoparticles to obtain a starch mixture;
[0007] S20. preparing a nanofiber membrane by electrospinning the starch mixture;
[0008] S30. Mix palm wax, dispersant and silicon dioxide, and spray them on the fiber membrane to obtain a nanofiber cling film.
[0009] In one embodiment, in step S10, the step of providing octenyl succinate starch ester-tannic acid-selenium nanoparticles comprises the following steps:
[0010] S11, mixing the octenyl succinate starch ester solution, the selenious acid solution and ascorbic acid to obtain octenyl succinate starch ester-selenium nanoparticles;
[0011] S12, mixing the octenyl succinate starch ester-selenium nanoparticles with tannic acid to obtain octenyl succinate starch ester-tannic acid-selenium nanoparticles.
[0012] In one embodiment, in step S11, the mass ratio of the octenyl succinate starch ester solution, the selenous acid solution and the ascorbic acid is 1:(9-10):(40-50); and / or,
[0013] In step S12, the mass ratio of octenyl succinate starch ester-selenium nanoparticles to tannic acid is (4-5):3.
[0014] In one embodiment, in step S10, in the octenyl succinate starch ester-tannic acid-selenium nanoparticles, the content of selenium nanoparticles is 133-135 μg / mL; and / or,
[0015] In step S10, the mass ratio of octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester-tannic acid-selenium nanoparticles is 375:375:2500:(1-10).
[0016] In one embodiment, in step S20, the ambient temperature of the electrospinning is 25-30° C., the relative humidity of the ambient is 40%, and the electrospinning time is 24 hours.
[0017] In one embodiment, step S30 includes:
[0018] S31, mixing palm wax, n-hexane and silicon dioxide particles to obtain a palm wax / silicon dioxide particle mixed solution;
[0019] S32, spraying the mixed solution onto the nanofiber film to obtain the nanofiber food preservative film.
[0020] In one embodiment, in step S31, the mass ratio of palm wax, n-hexane and silica particles is (5-7):1:(8-12)
[0021] In step S32, the mixed liquid is sprayed at a distance of 15 cm from the nanofiber membrane, the number of sprayings is 20 times, and the mass of palm wax / silicon dioxide particles on the nanocellulose membrane is 0.3 g.
[0022] The present invention also provides a nanofiber cling film, which is prepared according to the above-mentioned method for preparing the nanofiber cling film.
[0023] The present invention also provides an application of a nanofiber cling film in food preservation and food packaging, wherein the nanofiber cling film comprises the nanofiber cling film as described above.
[0024] The present invention also provides a method for recycling a nanofiber cling film, wherein the nanofiber cling film comprises the nanofiber cling film as described above;
[0025] The recycling method of the nanofiber food preservative film comprises the following steps: mixing the nanofiber food preservative film with water, filtering, and obtaining a recyclate, wherein the recyclate comprises palm wax / silicon dioxide particles and octenyl succinate starch ester-tannic acid-selenium nanoparticles.
[0026] The technical solution of the present invention adopts octenyl succinate starch ester-tannic acid-selenium nanoparticles, pullulan and octenyl succinate starch ester to prepare a nanofiber film, and the octenyl succinate starch ester-tannic acid-selenium nanoparticles are used to enhance the barrier property, mechanical property, antioxidant property and antibacterial property of the nanofiber food preservative film; palm wax and silicon dioxide are sprayed on the nanofiber film, so that the palm wax / silicon dioxide particle coating on the nanofiber film gives the nanofiber food preservative film super-hydrophobicity, so that the prepared nanofiber food preservative film can effectively prevent fruits from rotting and prolong the shelf life of fruits, and the prepared nanofiber food preservative film can be degraded in water, so that the coating and selenium nanoparticles can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 This is a scanning electron microscope image of the nanofiber cling film provided in Example 6 of the present invention;
[0029] Figure 2 The scanning electron microscope images of the nanofiber cling film provided in Examples 1 to 5 of the present invention and Comparative Example 1;
[0030] Figure 3 The permeability diagram of the nanofiber cling film provided in Examples 1 to 6 of the present invention and Comparative Example 1;
[0031] Figure 4 The water contact angle diagram of the nanofiber cling film provided in Examples 1 to 6 of the present invention and Comparative Example 1;
[0032] Figure 5 A graph showing the free radical scavenging rate of the nanofiber cling film provided in Examples 1 to 6 of the present invention and Comparative Example 1;
[0033] Figure 6This is a graph showing the performance of the nanofiber cling film provided in Examples 1 to 6 of the present invention and Comparative Example 1 in inhibiting Staphylococcus aureus and Escherichia coli;
[0034] Figure 7 This is a diagram showing the appearance changes of the nanofiber cling film provided in Example 1 and Comparative Example 1 of the present invention after being used to preserve strawberries;
[0035] Figure 8 This is a graph showing changes in strawberry indicators after the nanofiber cling film provided in Example 1 and Comparative Example 1 of the present invention is used to preserve strawberries;
[0036] Fig. 9 The recovery rate of the palm wax / silicon dioxide coating of the nanofiber cling film provided in Example 6 of the present invention.
[0037] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0038] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.
[0039] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.
[0040] Currently, supramolecular engineering strategies based on tannic acid are applied to construct various two-dimensional functional metal-phenol network materials, such as capsules or membranes, and are widely used in three-dimensional supramolecular nanomedicines. However, these studies are all based on the assembly of tannic acid, and its modification of the interface is hydrophilic, and its hydrophobic performance is poor.
[0041] In view of this, the present invention proposes a method for preparing a nanofiber cling film, comprising the following steps: S10. providing octenyl succinate starch ester-tannic acid-selenium nanoparticles, mixing octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester-tannic acid-selenium nanoparticles to obtain a starch mixture; S20. preparing a nanofiber membrane from the starch mixture by an electrospinning method; S30. mixing palm wax, a dispersant and silicon dioxide, and spraying the mixture on the fiber membrane to obtain a nanofiber cling film.
[0042] The technical solution of the present invention adopts octenyl succinate starch ester-tannic acid-selenium nanoparticles, pullulan and octenyl succinate starch ester to prepare a nanofiber film, and the octenyl succinate starch ester-tannic acid-selenium nanoparticles are used to enhance the barrier property, mechanical property, antioxidant property and antibacterial property of the nanofiber food preservative film; palm wax and silicon dioxide are sprayed on the nanofiber film, so that the palm wax / silicon dioxide particle coating on the nanofiber film gives the nanofiber food preservative film super-hydrophobicity, so that the prepared nanofiber food preservative film can effectively prevent fruits from rotting and prolong the shelf life of fruits, and the prepared nanofiber food preservative film can be degraded in water, so that the coating and selenium nanoparticles can be reused.
[0043] It should be noted that electrospinning is a method for preparing nanofiber membranes, which utilizes high electrostatic force to stretch the viscoelastic jet generated from a polymer solution to obtain nanofibers and nanofiber membranes.
[0044] Specifically, in step S10, when mixing the octenyl succinate starch ester (OSAS), pullulan (PUL), water and octenyl succinate starch ester-tannic acid-selenium nanoparticles (OSAS-TA-SeNPs), OSAS and PUL must be mixed with water first, and then OSAS-TA-SeNPs are added; in step S30, when mixing palm wax and silica particles, the palm wax is first dissolved in n-hexane, and then the silica particles are dispersed therein.
[0045] In one embodiment, in step S10, the step of providing octenyl succinate starch ester-tannic acid-selenium nanoparticles includes the following steps: S11, mixing octenyl succinate starch ester solution, selenous acid solution and ascorbic acid to obtain octenyl succinate starch ester-selenium nanoparticles; S12, mixing the octenyl succinate starch ester-selenium nanoparticles with tannic acid to obtain octenyl succinate starch ester-tannic acid-selenium nanoparticles.
[0046] The technical solution of the present invention adopts ascorbic acid as a reducing agent to reduce selenium ions to selenium element, thereby preparing selenium nanoparticles, and adopts octenyl succinate starch ester as a carrier to improve the stability of the selenium nanoparticles; and adopts tannic acid to mix with the octenyl succinate starch ester-selenium nanoparticles so that the tannic acid molecules can interact with the octenyl succinate starch ester-selenium nanoparticles, thereby further improving the hydrophobicity of the octenyl succinate starch ester-tannic acid-selenium nanoparticles.
[0047] In one embodiment, in step S11, the mass ratio of octenyl succinate starch ester solution, selenious acid solution and ascorbic acid is 1:(9-10):(40-50); and / or, in step S12, the mass ratio of octenyl succinate starch ester-selenium nanoparticles and tannic acid is (4-5):3.
[0048] The technical solution of the present invention can efficiently generate uniformly dispersed selenium nanoparticles by controlling the mass ratio between octenyl succinate starch ester, selenous acid and ascorbic acid, while ensuring the size and morphology consistency of the nanoparticles, thereby improving its stability and thus improving the hydrophobicity of the nanofiber membrane; by adjusting the mass ratio of octenyl succinate starch ester-selenium nanoparticles to tannic acid, the combination of tannic acid and selenium nanoparticles can be effectively promoted to form a more stable composite structure, further enhancing the stability of the nanofiber membrane, while improving the antibacterial and antioxidant properties of the nanofiber membrane. Specifically, the octenyl succinate starch ester solution and the selenous acid solution are first uniformly mixed, and then ascorbic acid as a reducing agent is added; before the octenyl succinate starch ester-selenium nanoparticles are mixed with tannic acid, they must be cleaned by dialysis. In order to make the reaction more sufficient, during the reaction, stirring and other means are used to promote the full contact of the raw materials, and then the reaction is fully reacted. In some embodiments, in order to make the reaction more sufficient, during the reaction, stirring and other means are used to promote the full contact of the raw materials, and then the reaction is fully reacted.
[0049] In one embodiment, in step S10, in the octenyl succinate starch ester-tannic acid-selenium nanoparticles, the content of selenium nanoparticles is 133-135 μg / mL; and / or, in step S10, the mass ratio of octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester-tannic acid-selenium nanoparticles is 375:375:2500:(1-10).
[0050] The technical solution of the present invention adjusts the content of selenium nanoparticles to 133-135 μg / mL to control the content of selenium in OSAS-TA-SeNPs, thereby improving the antibacterial and antioxidant capabilities of the nanofiber membrane. If the concentration is too high, the effect is the same as that achieved by the existing concentration, and excessive addition will cause unnecessary waste; the mass ratio of OSAS, PUL, water and OSAS-TA-SeNPs is 375:375:2500:(1-10) to form a stable composite material, ensure the stability of the material under different application conditions, and further improve the hydrophobicity of the prepared nanofiber membrane.
[0051] Specifically, since selenium nanoparticles are gradually formed during the reaction, whether the reaction is completed can be determined by the solution turning red, and the judgment method is simple and quick.
[0052] In one embodiment, in step S20, the ambient temperature of the electrospinning is 25-30° C., the relative humidity of the ambient is 40%, and the electrospinning time is 24 hours.
[0053] The technical solution of the present invention controls the ambient temperature at 25-30°C and the relative humidity at 40%. These conditions ensure the stability of the materials and the consistency of the fibers during the spinning process, help to form a uniform fiber structure, and thus improve the quality and performance of the final product; and the electrospinning time is set to 24 hours to ensure that all materials are fully spun, thereby obtaining a fiber membrane with good surface properties.
[0054] In one embodiment, step S30 includes: S31, mixing palm wax, n-hexane and silica particles to obtain a palm wax / silicon dioxide particle mixed solution; S32, spraying the mixed solution onto the nanofiber film to obtain the nanofiber food preservative film.
[0055] The technical solution of the present invention forms a protective layer on the surface of the nanofiber by mixing palm wax, n-hexane and silicon dioxide particles to form a mixed liquid and spraying it on the nanofiber membrane. Palm wax, as a natural wax, can provide good moisture-proof and oxygen-isolating properties, which helps to extend the shelf life of food; by adding silicon dioxide particles, the mechanical strength and stability of the membrane are improved, and the barrier properties of the membrane are also increased to prevent oxygen, moisture, etc. from entering, further improving the preservation effect of the nanofiber membrane.
[0056] In one embodiment, in step S31, the mass ratio of palm wax, n-hexane and silicon dioxide particles is (5-7):1:(8-12); and / or,
[0057] In step S32, the mixed liquid is sprayed at a distance of 15 cm from the nanofiber membrane, the number of sprayings is 20 times, and the mass of palm wax / silicon dioxide particles on the nanocellulose membrane is 0.3 g.
[0058] The technical solution of the present invention ensures the stability of the mixed liquid by controlling the mass ratio of palm wax, n-hexane and silicon dioxide particles to (5-7):1:(8-12), so as to form a uniform coating during spraying, wherein palm wax, as the main component of the coating, provides good moisture-proof and oxygen-isolating properties, and helps to extend the shelf life of food, and the addition of silicon dioxide particles helps to improve the mechanical strength and stability of the film, and also increases the barrier performance of the film; by controlling the spraying distance and number of times, the uniformity and stability of the coating can be effectively improved, and a uniform protective layer can be ensured to be formed on the surface of the nanofiber membrane; when the number of spraying is 5, 10, and 15 times, the nanofiber membrane is hydrophobic, but its hydrophobic property does not reach super-hydrophobicity, and when the number of spraying exceeds 20 times, the contact angle is substantially the same as that at 20 times, so 20 times of spraying is better, and too much will cause unnecessary production waste.
[0059] The present invention also provides a nanofiber cling film, which is prepared according to the above-mentioned method for preparing the nanofiber cling film, and is used for food packaging.
[0060] Since the nanofiber cling film includes all technical solutions of the preparation method of the nanofiber cling film, it also has all the beneficial effects brought by the above solutions, which will not be described one by one here.
[0061] The present invention also provides an application of a nanofiber cling film in food preservation and food packaging, wherein the nanofiber cling film comprises the nanofiber cling film as described above.
[0062] Since the application of the nanofiber cling film in food preservation and food packaging includes all technical solutions of the preparation method of the nanofiber cling film, it also has all the beneficial effects brought by the above solutions, which will not be described one by one here.
[0063] The present invention also proposes a method for recycling nanofiber cling film, wherein the nanofiber cling film includes the nanofiber cling film as described above; the method for recycling the nanofiber cling film includes the following steps: mixing the nanofiber food cling film with water, filtering, and obtaining a recyclate, wherein the recyclate includes palm wax / silicon dioxide particles and octenyl succinate starch ester-tannic acid-selenium nanoparticles.
[0064] It should be noted that the solid obtained by filtration, i.e., the recyclate, includes palm wax / silicon dioxide particles and octenyl succinate starch ester-tannic acid-selenium nanoparticles, and the recyclate can be separated and purified before reuse; in addition, the filtrate after filtration also contains pullulan and octenyl succinate starch ester, and its purification efficiency and utilization value are relatively low.
[0065] Specifically, the nanofiber food preservative film is put into water and stirred to dissolve, the palm wax / silicon dioxide particle coating floating on the water surface can be recovered by filtering, and the octenyl succinate starch ester-tannic acid-selenium nanoparticles in the filtrate can also be reused.
[0066] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0067] Example 1
[0068] This embodiment provides a nanofiber cling film, and the steps of the preparation method thereof are as follows:
[0069] 1. Dissolve 1.5 g of octenyl succinate starch ester and 1.5 g of pullulan in 8 mL of deionized water, heat and stir at 100°C for 1 to 2 h until the octenyl succinate starch ester and pullulan are completely dissolved to obtain an octenyl succinate starch ester-pullulan solution;
[0070] 2. A dispersion of 2 mL of OSAS-TA-SeNPs with a concentration of 956 μg / mL was mixed with 8 mL of octenyl succinate starch-pullulan solution, and magnetically stirred for 12 h or more to obtain a mixed solution, in which the mass ratio of starch, pullulan and OSAS-TA-SeNPs was 375:375:1.98. After stirring, the bubbles were removed by ultrasonic treatment;
[0071] 3. Finally, 5 ml of the prepared 10 ml solution was poured into a syringe, and the nanofiber cling film was prepared by electrospinning technology, which was marked as SNFs / Se 5 in the figure;
[0072] The preparation method of OSAS-TA-SeNPs is as follows: dissolve 1 mL of 75 mM ascorbic acid in 8 mL of 0.3 mg / mL OSAS solution, add 1 mL of 25 mM H2SeO3 solution, and stir continuously to form a stable red solution, namely OSAS-SeNPs, dialyze to remove excess ascorbic acid, and add TA to the OSAS-SeNPs solution after dialysis to form OSAS-TA-SeNPs, wherein the mass ratio of octenyl succinic acid starch ester, selenious acid and ascorbic acid is 3:28:132, and the concentration of TA in the solution is maintained at 0.3 mg / mL, so that the mass ratio of OSAS-TA-SeNPs and tannic acid is 4.91:3.
[0073] Example 2
[0074] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of Example 1, except that in Example 2, the concentration of OSAS-TA-SeNPs added is 1912 μg / mL, the volume is 2 mL, and after electrospinning, a nanofiber cling film is obtained, which is denoted as SNFs / Se 10 in the figure.
[0075] Example 3
[0076] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of Example 1, except that in Example 3, the concentration of OSAS-TA-SeNPs added is 2868 μg / mL, and the volume is 2 mL. After electrospinning, a nanofiber cling film is obtained, which is denoted as SNFs / Se 15 in the figure.
[0077] Example 4
[0078] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of Example 1, except that in Example 4, the concentration of OSAS-TA-SeNPs added is 3823 μg / mL, the volume is 2 mL, and after electrospinning, a nanofiber cling film is obtained, which is denoted as SNFs / Se 20 in the figure.
[0079] Example 5
[0080] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of Example 1, except that in Example 5, the concentration of OSAS-TA-SeNPs added is 4779 μg / mL, the volume is 2 mL, and after electrospinning, a nanofiber cling film is obtained, which is denoted as SNFs / Se 25 in the figure.
[0081] Example 6
[0082] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of embodiment 4, except that, after the nanofiber cling film is prepared in embodiment 6, palm wax / silicon dioxide particles are sprayed on the surface of the SNFs / Se 20 film, comprising the following steps:
[0083] Mix 0.6g palm wax and 0.1g n-hexane, heat and dissolve, then disperse 1g silica particles in the hot wax solution;
[0084] The palm wax / silica particle mixture was sprayed 20 times at a distance of 15 cm from the SNFs / Se 20 membrane. The mass of palm wax / silica particles on the nanocellulose membrane was 0.3 g, and a superhydrophobic nanofiber cling film was prepared, which was denoted as SHFs in the figure.
[0085] Comparative Example 1
[0086] This embodiment provides a nanofiber cling film, and its preparation method is similar to that of embodiment 1, except that no OSAS-TA-SeNPs dispersion is added to obtain the nanofiber cling film, which is denoted as SNFs in the figure.
[0087] Performance Testing and Results
[0088] The surface microstructures of the nanofiber cling films prepared in Examples 1 to 6 and Comparative Example 1 were observed using a scanning electron microscope, and the scanning electron microscope images were recorded as follows: Figure 1 , Figure 2 See Figure 1 In Example 6, after the surface of the nanofiber cling film was sprayed with the palm wax / silicon dioxide particle mixture, it was observed that the silicon dioxide particles were attached to the film surface by the palm wax, thus presenting an obvious rough structure. After this treatment, a super-hydrophobic state can be effectively generated to obtain a super-hydrophobic interface. Figure 2 , wherein Figures a to f correspond to the surfaces of the nanofiber cling films of comparative example 1, embodiment 1, embodiment 2, embodiment 3, embodiment 4 and embodiment 5, respectively. It can be found that the microscopic morphologies of embodiments 1 to 5 are similar to those of comparative example 1, octenyl succinate starch ester-tannic acid-selenium nanoparticles do not affect the film morphology, all nanofiber cling films have a smooth surface, and the electrospun fibers are tubular in morphology, relatively uniform and without beads, presenting a network structure with good continuity.
[0089] The water vapor permeability and carbon dioxide permeability tests were performed on Examples 1 to 6 and Comparative Example 1. The experimental results are as follows: Figure 3 As shown, Figure 3Figure (a) is a statistical graph of water vapor transmission rate, and Figure (b) is a statistical graph of carbon dioxide transmission rate. As the amount of octenyl succinate starch ester-tannic acid-selenium nanoparticles gradually increases, the barrier of nanofiber cling film to water vapor and carbon dioxide is enhanced, and palm wax / silicon dioxide particles have no negative impact on the barrier property.
[0090] The contact angle was used to characterize the water contact angle of Examples 1 to 6 and Comparative Example 1. The experimental results are as follows: Figure 4 As shown, the nanofiber cling film of comparative example 1 and examples 1 to 5 are all hydrophilic with a water contact angle of 0°, while the water contact angle of example 6 after being coated with palm wax / silicon dioxide particles is 151°, indicating that the nanofiber cling film can achieve superhydrophobicity.
[0091] The antioxidant activity of the nanofiber cling film of Examples 1 to 6 and Comparative Example 1 was tested by DPPH free radical scavenging rate. The experimental results are as follows: Figure 5 As shown, Comparative Example 1 does not have antioxidant properties, and the increase in its mass does not improve the free radical scavenging rate. The addition of octenyl succinate starch ester-tannic acid-selenium nanoparticles significantly improves the DPPH free radical scavenging activity of the nanofiber preservative film, and the scavenging activity is in a positive feedback relationship with the selenium content. After super-hydrophobic treatment, the DPPH free radical scavenging amount of Example 6 is slightly reduced compared with Example 4, because the hydrophobic layer does not have antioxidant capacity, but it occupies weight, reduces the amount of octenyl succinate starch ester-tannic acid-selenium nanoparticles that can scavenge free radicals, but still maintains a higher DPPH free radical scavenging activity.
[0092] The antibacterial activities of Examples 1 to 6 and Comparative Example 1 against Escherichia coli and Staphylococcus aureus are as follows: Figure 6 As shown, the antibacterial effect of comparative example 1 on the two bacteria is very small, while the antibacterial activity of examples 1 to 5 is significantly increased, and increases with the increase of SeNPs concentration. There is no significant difference in the antibacterial activity of example 6 and example 4 on Escherichia coli and Staphylococcus aureus, and the antibacterial rate is more than 99%.
[0093] Example 6 and Comparative Example 1 were used in a fruit preservation experiment. The results are as follows Figure 7 , Figure 8 As shown, Figure 8 Figure (a) is a graph showing the change in the spoilage rate of strawberries, and Figure (b) is a graph showing the change in the weight loss rate of strawberries. The introduction of octenyl succinate starch ester-tannic acid-selenium nanoparticles and palm wax / silicon dioxide particles in Example 6 enhances the antibacterial, antioxidant, and hydrophobic properties of the nanocellulose food preservative film, further improving the fruit preservation effect. The nanofiber preservative film can extend the shelf life of strawberries to 5 days.
[0094] After Example 6 was stirred in water, the recovery rate of the palm wax / silicon dioxide coating was tested. The results were as follows: Fig. 9 As shown, the recovery rate of palm wax / silica particle coating is 80.65±6.88%, and the nanofiber cling film can be reused through degradation in water.
[0095] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a nanofiber cling film, characterized in that: The following steps are involved: S10. Providing octenyl succinate starch ester - tannic acid - selenium nanoparticles, mixing octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester - tannic acid - selenium nanoparticles to obtain a starch mixture; S20. preparing a nanofiber membrane by electrospinning the starch mixture; S30. Mix palm wax, dispersant and silicon dioxide, and spray them on the fiber membrane to obtain a nanofiber cling film.
2. The method for preparing the nanofiber cling film according to claim 1, characterized in that: In step S10, the step of providing octenyl succinate starch ester-tannic acid-selenium nanoparticles comprises the following steps: S11, mixing the octenyl succinate starch ester solution, the selenious acid solution and ascorbic acid to obtain octenyl succinate starch ester-selenium nanoparticles; S12, mixing the octenyl succinate starch ester-selenium nanoparticles with a tannic acid dispersion to obtain octenyl succinate starch ester-tannic acid-selenium nanoparticles.
3. The method for preparing the nanofiber cling film according to claim 2, characterized in that: In step S11, the mass ratio of the octenyl succinate starch ester solution, the selenous acid solution and the ascorbic acid is 1:(9-10):(40-50); and / or, In step S12, the mass ratio of octenyl succinate starch ester-selenium nanoparticles to tannic acid is (4-5):
3.
4. The method for preparing the nanofiber cling film according to claim 1, characterized in that: In step S10, in the octenyl succinate starch ester-tannic acid-selenium nanoparticles, the content of selenium nanoparticles is 133-135 μg / mL; and / or, In step S10, the mass ratio of octenyl succinate starch ester, pullulan, water and octenyl succinate starch ester-tannic acid-selenium nanoparticles is 375:375:2500:(1-10).
5. The method for preparing the nanofiber cling film according to claim 1, characterized in that: In step S20, the ambient temperature of the electrospinning is 25-30° C., the relative humidity is 40%, and the electrospinning time is 24 hours.
6. The method for preparing the nanofiber cling film according to claim 1, characterized in that: Step S30 includes: S31, mixing palm wax, n-hexane and silicon dioxide particles to obtain a palm wax / silicon dioxide particle mixed solution; S32, spraying the mixed solution onto the nanofiber film to obtain the nanofiber food preservative film.
7. The method for preparing the nanofiber cling film according to claim 6, characterized in that: In step S31, the mass ratio of palm wax, n-hexane and silica particles is (5-7):1:(8-12); and / or, In step S32, the mixed liquid is sprayed at a distance of 15 cm from the nanofiber membrane, the number of sprayings is 20 times, and the mass of palm wax / silicon dioxide particles on the nanocellulose membrane is 0.3 g.
8. A nanofiber cling film, characterized in that: The nanofiber cling film is prepared according to the method for preparing the nanofiber cling film according to any one of claims 1 to 7.
9. Application of a nanofiber cling film in food preservation and food packaging, characterized in that: The nanofiber cling film comprises the nanofiber cling film as claimed in claim 8.
10. A method for recycling nanofiber cling film, characterized in that: The nanofiber cling film comprises the nanofiber cling film as claimed in claim 8; The recycling method of the nanofiber food preservative film comprises the following steps: mixing the nanofiber food preservative film with water, filtering, and obtaining a recyclate, wherein the recyclate comprises palm wax / silicon dioxide particles and octenyl succinate starch ester-tannic acid-selenium nanoparticles.
Citation Information
Cited By
Preparation and application of composite fresh-keeping pad capable of accurately regulating and controlling storage and fresh-keeping effects of picked cherries
CN120382706A