Black photoresist composition, preparation method thereof and black frame manufacturing process

By using black photoresist compositions with components such as bisphenol fluorene acrylic resin and β-H atomic tertiary amine resin, the problem of uneven film formation of black photoresist on the arc-surface cover plate is solved, and high Black bezel with light shading and weather resistance, suitable for smart car display covers.

CN119045278APending Publication Date: 2024-11-29SHENZHEN BRTHRBORDER SEMICON MATERIALS CO LTD

Patent Information

Application Number
CN202410464312.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing black photoresist is prone to shrinkage when spraying on the curved cover plate, uneven film formation and insufficient light shading rate, resulting in weak film surface and inability to meet the requirements.

Method used

A black photoresist composition is adopted, including bisphenol fluorene acrylic resin, tertiary amine resin containing β-H atoms, photocuring resin monomers, photoinitiators, thermal initiators, black colorants and polarities Organic solvents form high-quality black borders through specific preparation methods and process flows.

Benefits of technology

It is achieved to form a uniform and weather-resistant black frame on the arc cover plate, with a development accuracy of 3μm, a high light shading rate and a low film thickness. It has the advantages of resistant to erosion of acid and alkali, solvents and film stripping liquids, and adapts to high-temperature and high-humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119045278A_ABST
    Figure CN119045278A_ABST
Patent Text Reader

Abstract

The invention discloses a black photoresist composition, a preparation method thereof and a black frame manufacturing process, and belongs to the technical field of photoresist. The black photoresist composition is prepared from the following components in parts by weight: 2 to 20 parts of bisphenol fluorene acrylic resin, 1 to 10 parts of tertiary amine resin containing beta to H atoms, 0.1 to 2 parts of auxiliary A, 0.2 to 5 parts of auxiliary B, 0.5 to 2 parts of photoinitiator, 5 to 10 parts of light-cured resin monomer, 10 to 50 parts of black coloring agent and 50 to 500 parts of polar organic solvent. The black photoresist is resistant to corrosion of acid and alkali, solvents, film stripping liquid and copper etching liquid after being formed and cured. The spraying adaptability on a cambered surface glass cover plate is good, the film forming uniformity is good, the minimum developing precision can reach 3 microns after a photoetching procedure, a black frame is free of burrs and sawteeth, and the characteristics of high shading rate and low film thickness are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photoresists, and in particular to a black photoresist composition and a preparation method thereof, and a black frame manufacturing process. Background Art

[0002] The edges of existing smart car display cover plates are often provided with patterned light-shielding films such as black matrix and black columnar spacers. The light-shielding film layer is the black frame of the smart car display cover plate. The black frame is used to prevent light leakage from the edge of the cover plate and block light.

[0003] At present, pad printing, UV curing ink and LDI photolithography can all form specific answers on flat cover plates. LDI photolithography uses black photoresist to spray on the curved cover plate, and the laser directly forms a black frame after imaging.

[0004] However, the application of flat-sprayed black photoresist on curved cover plates has certain limitations. Shrinkage holes will appear during film formation, and a good film surface cannot be formed. The uneven film surface causes the shading rate at the weak points of the film surface to fail to meet the requirements.

[0005] Therefore, improvements are needed in the black photoresist used in the spray coating of curved cover plates. Summary of the invention

[0006] The main purpose of the present invention is to provide a black photoresist composition, which aims to solve the technical problem that when a flat-sprayed black photoresist is applied on a curved cover plate, shrinkage holes will appear during film formation, a good film surface cannot be formed, and the film surface is uneven, resulting in the shading rate at the weak parts of the film surface failing to meet the requirements.

[0007] To achieve the above object, the present invention provides a black photoresist composition, which comprises an alkali-soluble photopolymer resin, a photocurable resin monomer, an auxiliary agent A, an auxiliary agent B, a photoinitiator, a thermal initiator, a black colorant, and a polar organic solvent;

[0008] Among them, the photopolymer resin includes two types of resins: bisphenol fluorene acrylic resin and tertiary amine resin containing β-H atoms;

[0009] In parts by weight, the black photoresist composition includes 2 to 20 parts of the bisphenol fluorene acrylic resin, 1 to 10 parts of the tertiary amine resin containing β-H atoms, 0.1 to 2 parts of auxiliary agent A, 0.2 to 5 parts of auxiliary agent B, 0.5 to 2 parts of the photoinitiator, 5 to 10 parts of the photocurable resin monomer, 10 to 50 parts of the black colorant and 50 to 500 parts of the polar organic solvent.

[0010] Preferably, the bisphenol fluorene acrylic resin is selected from one or more compounds shown in general formula (I);

[0011]

[0012] wherein n is an integer of 10 to 180; R1 and R3 are CH2; R2 and R4 are OH; X and W are A is selected from H or C1-2 alkyl.

[0013] A method for preparing a bisphenol fluorene acrylic resin, the preparation method comprising the following steps:

[0014] (a) Synthetic intermediate: A compound represented by structural formula (I-2) is produced by ring-opening polymerization of a monomer represented by structural formula (I-1) and an acrylic compound;

[0015]

[0016] (b) Synthesizing the product: Continue to dropwise add the acrylic acid compound to the intermediate of the above structural formula (I-2) under nitrogen to react to generate the structural formula (I);

[0017]

[0018] (c) Product post-treatment: When the reaction of the intermediate of formula (I-2) is completed by monitoring with a spot chromatography plate, the product is transferred to a round-bottom flask while hot for purification to obtain a milky white powder resin, which is then dried.

[0019] Specifically, in the above scheme, the acrylic compound is one of methacrylic acid, ethylacrylic acid, acrylic acid, benzyl acrylate, styrene, methyl methacrylate, butyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, tricyclo[5.2.1.02,6]dec-8-yl methacrylate, hydroxyethyl methacrylate, and hydroxybutyl acrylate.

[0020] In a further embodiment, in the above preparation method, the specific steps of preparing the intermediate in step (a) are: adding the acrylic compound to the monomer represented by the structural formula (I-1) in a molar ratio of 1:(2-4) between the monomer represented by the structural formula (I-1) and the acrylic compound, and then adding 1% tetramethylammonium chloride and 0.5% phenol in sequence, accounting for the total mass of the monomer represented by the structural formula (I-1) and the acrylic compound, and protecting with nitrogen at 90°C. After complete dissolution in 30 minutes, heating to 130°C and continuing the reaction, measuring the acid value during the reaction, stopping the reaction after the acid value of the solution is less than 2.0 mg, and distilling under reduced pressure to obtain the intermediate compound.

[0021] Preferably, the tertiary amine resin containing β-H atoms is selected from one or more compounds shown in general formula (II);

[0022]

[0023] Among them, R is A is selected from H or C1-2 alkyl; R1 is selected from -H, -CH3, R2 is selected from phenyl (II-1), benzyl (II-2), phenol (II-3)

[0024]

[0025] Preferably, the mass ratio of the bisphenol fluorene acrylic resin to the tertiary amine resin containing β-H atoms is in the range of 1:1 to 5:1.

[0026] Preferably, the photoinitiator is a carbazole oxime ester compound, and the photoinitiator is selected from one or more compounds shown in general formula (III);

[0027]

[0028] Wherein, R1 is selected from -H, -CH3, -CH2CH3, -CH2CH2CH3, R2 is selected from R3 is selected from -H, -CH3, , R4 is selected from -CH3, -CH2CH3, Preferably, the photoinitiator is:

[0029]

[0030] Preferably, the photocurable resin monomer is an acrylic resin, and the photocurable resin monomer is selected from one or more compounds shown in general formula (IV) (V);

[0031]

[0032] R1 is selected from R2 is selected from -H, The mass ratio of the photoinitiator to the photocurable resin monomer is in the range of 1:100 to 2:5.

[0033] Preferably, the photocurable resin monomer is an oligomer crosslinking agent containing olefinic double bonds, and the mass fraction of the photocurable resin monomer is 5-30 parts. The photocurable resin monomer is one or a mixture of pentaerythritol triacrylate, pentaerythritol tetraacrylate, 3-hydroxymethyl pentaerythritol triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate. The double bonds of the photocurable resin monomer are opened into a network crosslink in the presence of free radicals. If the mass fraction of the photocurable resin monomer is less than 5 parts, the crosslinking density of the photoresist will be insufficient, affecting the transformation of the material from thermoplastic resin to thermal curing. In the present invention, if the mass fraction of the photocurable resin monomer is higher than 30 parts, the photoresist will be excessively crosslinked, the CD value will be too high, and the CD Loss accuracy cannot be controlled. For the specific structure of the photocurable resin monomer, please refer to IV-1, IV-2, IV-3, V-1, and V-2.

[0034]

[0035] Preferably, the polar organic solvent is an organic aprotic polar solvent with medium polarity and strong polarity, generally one or more of ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, triethoxymethylacrylate, acetone, butanone, cyclohexanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate and butyl butyrate, and the mass ratio of the polar organic solvent to the photocurable resin monomer is between 5:1 and 100:1, preferably between 10:1 and 80:1, and more preferably between 20:1 and 70:1.

[0036] Preferably, the black colorant is selected from one or more of cyanine black, aniline black, carbon black, titanium black, and graphite black. In the present invention, the black colorant can also be a mixed organic pigment that is approximately black by mixing two or more pigments selected from red, blue, green, purple, yellow, cyanine, magenta, etc.

[0037] The black colorant is preferably carbon black particles, the size of the carbon black particles is 100 nm to 200 nm, and the mass ratio of the carbon black particles to the photocurable resin monomer is in the range of 10:1 to 1:1.

[0038] In the present invention, the carbon black particles can be, for example, Printex L6, Printex L, Printex 55, Printex 45, Printex 60, Extra Black 550, Extra Black 350, Printex 35, Extra Black 250, Printex 25, Extra Black 100, Printex 200, Hiblack 30, Hiblack 30L from Degussa, Raven 1255, Raven 1200, Raven 1170, Raven 1100 Ultra, Raven 1060 Ultra, Raven 1040, Raven 1035, Raven 1020, Raven 1000, Raven 890, Raven 860 Ultra, Raven 850, Raven 820, Raven 760 Ultra, Raven 460, Raven 450, Raven 410, Raven H.20, Raven8250B, Raven6800B, R99R, R250R, R330R, R400R, R660R, ML, DL430, etc. from CAB0T.

[0039] Preferably, the auxiliary agent A contains a perfluorinated substituted vinyl monomer, and the perfluorinated substituted vinyl monomer is selected from the compounds shown in the general formula (VI);

[0040]

[0041] Wherein, R1, R2, R3, R4 are selected from -CF3, One of them.

[0042] The specific structure of the perfluorinated substituted vinyl monomer is as follows:

[0043]

[0044] Preferably, the auxiliary agent B comprises at least one aromatic peroxide, and can undergo Cope elimination reaction with the β-H atom tertiary amine resin during post-photolithography curing to participate in photopolymerization curing, and the aromatic peroxide is selected from the compounds shown in general formula (VII);

[0045]

[0046] Wherein, R5 is selected from -Cl, -Br. The specific structure of the aromatic peroxide is as follows

[0047]

[0048] Preferably, the thermal initiator comprises a bisimidazole compound, and the bisimidazole compound is selected from the compounds shown in general formula (VIII);

[0049]

[0050] Wherein, R1 and R2 are independently selected from -H, methyl, ethyl, bromine or chlorine. The specific structure of the bisimidazole compound is as follows:

[0051]

[0052] Preferably, the preparation method comprises the following steps:

[0053] (1) preparing a black color paste: adding an organic solvent to a sand mill with zirconium balls of 0.05-0.1 mm in size to wet-grind the black colorant, and adding the bisphenol fluorene acrylic resin composition as a stabilizing resin during the grinding process to prepare a black color paste;

[0054] (2) preparing a photosensitive solution: mixing and dispersing the tertiary amine resin containing β-H atoms, the photocurable resin, the photoinitiator, the auxiliary agent A, the auxiliary agent B, and the polar organic solvent according to the formula amount into a solution and filtering the solution to obtain a photosensitive solution;

[0055] (3) Preparing a black photoresist composition: mixing the black color paste in step (1) and the photosensitive solution in step (2), and finally adding an organic solvent to adjust the viscosity, dispersing the mixture in a disperser to form a uniform solution, and filtering the mixture to obtain a black photoresist composition.

[0056] The present invention also provides the application of any of the above black photoresists in the field of curved cover plates for smart car displays.

[0057] The present invention also provides a process for manufacturing a black frame of a curved display glass base cover, comprising the following steps:

[0058] S11: spraying a first layer of the black photoresist as described above on the heat-bent curved glass substrate in the x direction by using an inkjet process, and pre-baking to form a black film with a thickness of 1-3 μm;

[0059] S12: using LDI laser direct writing lithography to partially expose the frame pattern, and after washing away the black photoresist in the frame through a developing process, the first layer of black frame is formed after post-baking and hardening;

[0060] S13: spraying a second layer of the above-mentioned black photoresist on the curved substrate with the first layer of black border in the y direction by inkjet process, and pre-baking to form a second layer of black film with a thickness of 1-3 μm;

[0061] S14: using LDI laser direct writing lithography again to partially expose the frame pattern, and after washing away the black photoresist in the frame through a development process, a second layer of black frame is formed after post-baking and hardening;

[0062] The post-baking temperature in S12 and S14 is 200-250°C.

[0063] The beneficial effects that can be achieved by the present invention are:

[0064] The black photoresist of the present invention is resistant to acid, alkali, solvent, film stripping liquid and copper etching liquid after film formation and curing; it is resistant to metal plating at 25-280°C; and the square resistance is stable at 5.0×10 12 The advantages of ohm / □ and above. It has good spraying adaptability on curved glass cover plates, good film uniformity, and its minimum development accuracy can reach 3μm after the photolithography process. The black frame is made without burrs and "sawtooths", and has the characteristics of high shading rate and low film thickness, which can reduce the amount used in production process applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a process flow chart of manufacturing a black frame of a curved display glass base cover plate of the present invention;

[0066] Figure 2 This is the process flow chart of black UV curing ink;

[0067] Figure 3 This is the process flow chart of pad printing ink;

[0068] Figure 4 This is a developed appearance image of a black frame prepared in Example 1 of the present invention;

[0069] Figure 5 This is a developed appearance image of a black frame prepared in Example 2 of the present invention;

[0070] Figure 6 The film thickness map of the black frame is prepared for the black UV curing ink process;

[0071] Figure 7 This is an appearance picture of the black film surface prepared in Example 2 of the present invention;

[0072] Figure 8 This is an appearance diagram of the weather resistance test of the black film surface prepared in Example 3 of the present invention;

[0073] Fig. 9 This is an appearance diagram of the black film surface prepared in Example 1 of the present invention being developed.

[0074] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0075] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0076] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is described in more detail below.

[0077] A black photoresist composition comprises an alkali-soluble photopolymer resin, a photocurable resin monomer, an auxiliary agent A, an auxiliary agent B, a photoinitiator, a thermal initiator, a black colorant, and a polar organic solvent.

[0078] Preferably, in parts by weight, the black photoresist composition comprises 2-20 parts of the bisphenol fluorene acrylic resin, 1-10 parts of the tertiary amine resin containing β-H atoms, 0.5-2 parts of the photoinitiator, 5-10 parts of the photocurable resin monomer, 10-50 parts of the black colorant and 50-500 parts of the polar organic solvent.

[0079] The photopolymerizable resin is a component that imparts photopolymerizability and film forming ability to the black photoresist. In view of photopolymerizability, alkali developability and adhesion, the photopolymerizable resin preferably contains an alkali-soluble epoxy acrylate having an unsaturated double bond. Further, in view of the performance of the black photoresist, the photopolymerizable resin preferably includes an alkali-soluble epoxy acrylate having a bisphenol fluorene group and a tertiary amine resin containing a β-H atom.

[0080] Preferably, the mass ratio of the bisphenol fluorene acrylic resin to the tertiary amine resin containing β-H atoms is in the range of 1:1 to 5:1.

[0081] The present invention also provides a method for preparing a bisphenol fluorene acrylic resin, which comprises the following steps:

[0082] (a) Synthetic intermediate: A compound represented by structural formula (I-2) is produced by ring-opening polymerization of a monomer represented by structural formula (I-1) and an acrylic compound;

[0083]

[0084] (b) Synthesizing the product: Continue to dropwise add the acrylic acid compound to the intermediate of the above structural formula (I-2) under nitrogen to react to generate the structural formula (I);

[0085]

[0086] (c) Product post-treatment: When the reaction of the intermediate of formula (I-2) is completed by monitoring with a spot chromatography plate, the product is transferred to a round-bottom flask while hot for purification to obtain a milky white powder resin, which is then dried.

[0087] Specifically, in the above scheme, the acrylic compound is one or more of methacrylic acid, ethylacrylic acid, acrylic acid, benzyl acrylate, styrene, methyl methacrylate, butyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, tricyclo[5.2.1.02,6]dec-8-yl methacrylate, hydroxyethyl methacrylate, and hydroxybutyl acrylate.

[0088] In a further embodiment, in the above-mentioned preparation method, the specific steps of preparing the intermediate in step (a) are as follows: according to the molar ratio of the monomer represented by structural formula (I-1) to the acrylic compound being 1:(2-4), the acrylic compound is added to the monomer represented by structural formula (I-1), and then 1% tetramethylammonium chloride and 0.5% phenol are added in sequence, accounting for the total mass of the monomer represented by structural formula (I-1) and the acrylic compound, and nitrogen is passed through at 90°C for protection. After complete dissolution in 30 minutes, the mixture is heated to 130°C and the reaction is continued. The acid value is measured during the reaction, and the reaction is stopped after the acid value of the solution is <2.0 mg, and distillation is carried out under reduced pressure to obtain the intermediate compound.

[0089] Of course, the epoxy resin having bisphenol fluorene groups can be purchased from the market, or can be prepared by referring to the method disclosed in the patent publication number CN110066382A.

[0090] Preferably, the bisphenol fluorene acrylic resin is selected from one or more compounds shown in general formula (I);

[0091]

[0092] wherein n is an integer of 10 to 180; R1 and R3 are CH2; R2 and R4 are OH; X and W are A is selected from H or C 1~2 of alkyl.

[0093] The tertiary amine resin containing β-H atoms is selected from one or more compounds shown in general formula (II);

[0094]

[0095] Among them, R is A is selected from H or C 1~2 An alkyl group; R1 is selected from -H, -CH3, R2 is selected from phenyl, benzyl, and phenol. The tertiary amine resin of the β-H atom has a CAS number of 13206-64-9. The specific structure of the tertiary amine resin of the β-H atom is as follows:

[0096]

[0097] Preferably, the mass ratio of the bisphenol fluorene acrylic resin to the tertiary amine resin containing β-H atoms is in the range of 1:1 to 5:1.

[0098] Preferably, the photoinitiator comprises a carbazole oxime ester compound, and the photoinitiator is selected from one or more compounds shown in the general formula (III).

[0099]

[0100] Wherein, R1 is selected from -H, -CH3, -CH2CH3, -CH2CH2CH3, R2 is selected from R3 is selected from -H, -CH3, R4 is selected from -CH3, -CH2CH3,

[0101] More preferably, the photocurable resin monomer is selected from one or more compounds shown in general formula (IV) (V);

[0102]

[0103] R1 is selected from R2 is selected from -H, The mass ratio of the photoinitiator to the photocurable resin monomer is in the range of 1:100 to 2:5.

[0104] Specifically, the photoinitiator containing the carbazole oxime ester compound may be OXE-2, and the OXE-2 may be purchased from a commercial product.

[0105] More preferably, the photocurable resin monomer is one or a mixture of pentaerythritol triacrylate, pentaerythritol tetraacrylate, 3-hydroxymethyl pentaerythritol triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate, and the double bonds are opened into a network crosslink in the presence of free radicals. In the present invention, if the mass fraction of the photocurable resin monomer is higher than 30 parts, it will cause the photoresist to be excessively crosslinked, the CD value is too high, and the CD Loss accuracy cannot be controlled. For the specific structure of the photocurable resin monomer, please refer to IV-1, IV-2, IV-3, V-1, and V-2.

[0106]

[0107] In the present invention, the photocurable resin monomer undergoes a photopolymerization reaction under the action of the photoinitiator, which is a carbazole oxime terpene compound, to generate an organic polymer structure with a three-dimensional cross-linked structure, which can improve the cross-linking degree of the photoresist, thereby improving the stability, corrosion resistance and heat resistance of the black frame.

[0108]

[0109] In the present invention, the black colorant is required to have better heat resistance, light resistance and solvent resistance. Preferably, the black colorant can be selected from black organic pigments such as perylene black, cyanine black, aniline black, etc. The black colorant can also be selected from two or more pigments such as red, blue, green, purple, yellow, cyanine, magenta, etc. to mix them to form a mixed color organic pigment that is approximately black. The black colorant can also be selected from one or more of carbon black, titanium black, and graphite black. The black colorant in the present invention can also be dispersed using a dispersant to obtain a better coloring effect. The dispersant can use anionic, cationic, nonionic, amphoteric, fluorine-based surfactants.

[0110] Preferably, the black colorant is carbon black particles, the size of the carbon black particles is 100nm-200nm, and the mass ratio of the carbon black particles to the photocurable resin monomer is in the range of 10:1 to 1:1.

[0111] In the present invention, the carbon black particles can be, for example, Printex L6, Printex L, Printex 55, Printex 45, Printex 60, Extra Black 550, Extra Black 350, Printex 35, Extra Black 250, Printex 25, Extra Black 100, Printex 200, Hiblack 30, Hiblack 30L from Degussa, Raven 1255, Raven 1200, Raven 1170, Raven 1100 Ultra, Raven 1060 Ultra, Raven 1040, Raven 1035, Raven 1020, Raven 1000, Raven 890, Raven 860 Ultra, Raven 850, Raven 820, Raven 760 from Colombia. 0ltra, Raven460, Raven450, Raven410, RavenH.20, Raven8250B, Raven6800B, R99R, R250R, R330R, R400R, R660R, ML, DL430, etc. from CAB0T.

[0112] Preferably, the auxiliary agent A contains a perfluorinated substituted vinyl monomer, and the perfluorinated substituted vinyl monomer is selected from the compounds shown in the general formula (VI);

[0113]

[0114] Wherein, R1, R2, R3, R4 are selected from -CF3, The specific structure of the perfluorinated substituted vinyl monomer is as follows:

[0115]

[0116] In the present invention, the additive A can significantly change the surface tension, viscosity, and leveling of the photoresist solvent system, and improve the construction performance of spraying. Moreover, under the action of the photoinitiator, a fluorine group is introduced during the polymerization process, similar to the following structure, and a small amount of fluorine-containing polymerized structure can improve the weather resistance of the light-shielding film layer formed after the black photoresist is cured.

[0117]

[0118] Preferably, the auxiliary agent B comprises at least one aromatic peroxide, and the aromatic peroxide is selected from the compounds shown in the general formula (VII);

[0119]

[0120] Wherein, R5 is selected from -F, -Cl, -Br. The specific structure of the aromatic peroxide is as follows:

[0121]

[0122] In the present invention, during the post-lithography curing process, the auxiliary agent B can undergo a Cope elimination reaction with the β-H atom tertiary amine resin to participate in photopolymerization curing. The β-H atom tertiary amine resin undergoes a Cope elimination reaction to obtain a resin containing an unsaturated bond, which can also be polymerized with the remaining unreacted photocurable resin monomer to increase the crosslinking density. When R1 in the structural formula shown in (II) is a C2 alkane carbon chain, if it occurs on the right side, an ethylene monomer will appear, participating in the photoactivated monomer, providing a smaller molecular weight for the copolymer, and the reaction is as follows:

[0123]

[0124] When R2 is C1 and H, there is no group on the right side that can undergo COPE elimination, so the reaction will occur on the left side, generating unsaturated olefins greater than 3 and providing a longer carbon chain. The reaction is as follows:

[0125]

[0126] Preferably, the thermal initiator comprises a bisimidazole compound, and the bisimidazole compound is selected from the compounds shown in general formula (VIII);

[0127]

[0128] Wherein, R1 and R2 are independently selected from -H, -Cl, and -Br. The specific structure of the biimidazole compound is as follows:

[0129]

[0130] The double bonds of the photocurable resin monomer are opened under the action of the biimidazole initiator to perform a thermal polymerization reaction:

[0131]

[0132] The left side of the right side of the reaction equation is the thermal polymerization of the short carbon chain ethylene generated after the COPE elimination reaction. The right side of the right side of the reaction equation is the long carbon chain, which can be distinguished from the COPE elimination above.

[0133] Specifically, the thermal initiator containing a bisimidazole compound may be B-CIM, and the B-CIM may be purchased from a commercial product.

[0134] In the present invention, an oxime ester photoinitiator and a biimidazole thermal initiator are used, and the combined use of the two improves the crosslinking density of the resin during polymerization.

[0135] Moreover, the use of the bisimidazole thermal initiator in the black frame manufacturing process allows the remaining unsaturated bonds of the black photoresist composition to continue to polymerize at the temperature of the post-baking process, thereby increasing the degree of cross-linking and optimizing the weather resistance of the cured film.

[0136] Preferably, the polar organic solvent is a ketone solvent or an ester solvent among non-protonic polar solvents, which has the advantages of low viscosity and complete removal after baking. Preferably, the polar organic solvent is an organic non-protonic polar solvent with medium polarity and strong polarity, generally ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, triethoxymethyl acrylate, acetone, butanone, cyclohexanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate or more, and the mass ratio with the photocurable resin monomer is between 5:1 and 100:1, preferably between 10:1 and 80:1, and more preferably between 20:1 and 70:1. It has a significant solvent effect on the Cope elimination reaction. The use of the non-protonic polar solvent can increase the rate of the Cope elimination reaction by up to one million times, thereby increasing the rate of the Cope elimination reaction to form double bonds. Furthermore, it is used to adjust the viscosity of black photoresist and improve its spraying construction performance.

[0137] The present invention also provides a method for preparing the above-mentioned photoresist composition, the preparation method comprising the following steps:

[0138] (1) preparing a black color paste: adding an organic solvent to a sand mill with zirconium balls of 0.05-0.1 mm in size to wet-grind the black colorant, and adding the bisphenol fluorene acrylic resin composition as a stabilizing resin during the grinding process to prepare a black color paste;

[0139] (2) preparing a photosensitive solution: mixing and dispersing the tertiary amine resin containing β-H atoms, the photocurable resin, the photoinitiator, the auxiliary agent A, the auxiliary agent B, and the polar organic solvent according to the formula amount into a solution and filtering the solution to obtain a photosensitive solution;

[0140] (3) Preparing a black photoresist composition: mixing the black color paste in step (1) and the photosensitive solution in step (2), and finally adding an organic solvent to adjust the viscosity, dispersing the mixture in a disperser to form a uniform solution, and filtering the mixture to obtain a black photoresist composition.

[0141] The present invention also provides an application of the above black photoresist in the field of smart car display curved cover plate. It is understandable that the black photoresist composition of the present invention can also be applied to other processes requiring black borders, such as tablet computers.

[0142] See also Figure 1The present invention also provides a process for manufacturing a black frame of a curved display glass base cover, comprising the following steps:

[0143] S11: spraying a first layer of the black photoresist as described above on the heat-bent curved glass substrate in the x direction by using an inkjet process, and pre-baking to form a black film with a thickness of 1-3 μm;

[0144] S12: using LDI laser direct writing lithography to partially expose the frame pattern, and after washing away the black photoresist in the frame through a developing process, the first layer of black frame is formed after post-baking and hardening;

[0145] S13: spraying a second layer of the black photoresist as described above in the y direction on the curved substrate with the first layer of black border by inkjet technology, and pre-baking to form a second layer of black film with a thickness of 1-3 μm;

[0146] S14: using LDI laser direct writing lithography again to partially expose the frame pattern, and after washing away the black photoresist in the frame through a development process, a second layer of black frame is formed after post-baking and hardening;

[0147] The post-baking temperature in S12 and S14 is 200-250°C.

[0148] Laser Direct Writing (LDI) is a technology that uses a computer-controlled laser beam to directly apply a fine pattern to a photoresist. Unlike traditional photolithography, it does not require a physical mask, which saves costs and shortens the production cycle. The working principle of this technology is to use a laser beam generated by a laser, which is controlled by a scanning system to accurately scan and expose the surface of the photoresist, so that the molecular chains on the photoresist undergo polymerization under laser irradiation to form the desired pattern. Laser direct writing photolithography can achieve high-precision pattern transfer and is suitable for special photolithography application scenarios with substrate warping or substrate deformation.

[0149] In the black frame manufacturing process of the present invention, since the LDI laser direct writing process is adopted, the energy is lower than that of the black UV curing ink process, and the resin in the black photoresist composition cannot be completely polymerized and cured. However, the use of the biimidazole thermal initiator in the present application enables the black photoresist composition to continue to polymerize the remaining unsaturated bonds at the temperature of the post-baking process in the black frame manufacturing process, and secondary curing, thereby improving the degree of crosslinking and optimizing the weather resistance of the film layer after curing. Moreover, the combination of the oxime ester photoinitiator and the biimidazole thermal initiator improves the crosslinking density of the resin during polymerization.

[0150] In summary, in the present invention, the bisphenol fluorene acrylic resin, the tertiary amine resin containing β-H atoms, and the photocurable resin monomer undergo a polymerization reaction during the LDI laser direct writing process under the action of the photoinitiator and the thermal initiator of the auxiliary agent A and the auxiliary agent B to finally obtain a black frame. The aromatic peroxide in the auxiliary agent B can undergo a Cope elimination reaction with the β-H atom tertiary amine resin and participate in photopolymerization curing. At the same time, in the post-baking process, a thermal polymerization reaction occurs under the diimidazole thermal initiator, and the tertiary amine resin containing β-H atoms undergoes cross-linking polymerization with the auxiliary agent A, introducing fluorine groups, improving the weather resistance of the shading film layer formed after curing, improving the cross-linking density of the resin, and optimizing the performance after curing. Moreover, the resin containing unsaturated bonds obtained by the Cope elimination reaction of the β-H atom tertiary amine resin can also be polymerized with the remaining unreacted photocurable resin monomer to improve the cross-linking density. The polar solvent is an aprotic polar solvent. The use of the aprotic polar solvent can increase the Cope elimination reaction rate by up to a million times.

[0151] Finally, the black photoresist of the present invention has the advantages of acid and alkali resistance, solvent resistance, film stripping liquid, and copper etching liquid resistance after film formation and curing; metal plating resistance at 25-280℃; and stable sheet resistance at 5.0×10 12 The advantages of ohm / □ and above. It has good spraying adaptability on curved glass cover plates, good film uniformity, and its minimum development accuracy can reach 3μm after the photolithography process. The black frame is made without burrs and "sawtooths", and has the characteristics of high shading rate and low film thickness, which can reduce the amount used in production process applications.

[0152] Example 1

[0153] The present embodiment provides a black photoresist composition, which includes, in parts by weight, 100 parts of the bisphenol fluorene acrylic resin, 50 parts of the β-H atom tertiary amine resin, 5 parts of the photoinitiator b-1, 5 parts of the thermal initiator b-2, 50 parts of the photocurable resin monomer, 180 parts of the carbon black colorant, 50 parts of the solvent e-1, 50 parts of the solvent e-2, 100 parts of the solvent e-3, 0.2 parts of the auxiliary agent A, and 2 parts of the auxiliary agent B.

[0154] An organic solvent is added to a sand mill with zirconium balls of 0.05-0.1 mm in size to wet-grind the black colorant, and the bisphenol fluorene acrylic resin composition is added as a stabilizing resin during the grinding process to obtain a black color paste.

[0155] The tertiary amine resin containing β-H atoms, the photocurable resin, the photoinitiator, the auxiliary agent A, the auxiliary agent B, and the polar organic solvent are mixed and dispersed into a solution according to the formula amount, and then filtered to obtain a photosensitive solution.

[0156] The black color paste and the photosensitive liquid are mixed, and finally an organic solvent is added to adjust the viscosity, and the mixture is dispersed into a uniform solution in a disperser, and filtered to obtain a black photoresist composition.

[0157] Embodiments 2 to 12

[0158] A black photoresist was prepared in the same manner as in Example 1, except that the composition ratio shown in Table 1 was used.

[0159] Table 1:

[0160]

[0161] The black photoresist compositions obtained in Examples 1 to 12 were respectively spin-coated on glass substrates and baked at 100° C. for 2 min to form a film with a thickness of less than 5 μm on the glass substrate. The glass substrate was then irradiated with a photomask at 60 mJ / cm 2 The layers were exposed to an energy of , and then developed in a 0.045% KOH solution for 90 seconds. After the development was completed, they were baked at 200° C. for 30 minutes to obtain black photoresist composition coatings 1 to 12.

[0162] Comparative Example 1

[0163] Black UV curing ink process

[0164] S21. Coat a first layer of black photoresist on a flat glass substrate using a coating process, and pre-bake to form a black film with a thickness of 1-3 μm, wherein the black photoresist is a commercially available product.

[0165] S22. Use Masker to mask the non-exposed area and expose the area outside the Masker.

[0166] S23, after the black photoresist in the frame is washed away by a development process, a first layer of black frame is formed after post-baking and hardening.

[0167] See also Figure 2 and Figure 6 The film thickness of the black border prepared by the black UV curing ink process reaches 11.7um.

[0168] Comparative Example 2

[0169] Pad printing ink process

[0170] S31, cleaning and drying the curved display glass base cover.

[0171] S32, use the pad printing gun to apply the pad printing ink to the black light-shielding area where the film needs to be formed, and then post-bake it for curing. For details of the pad printing ink process, please refer to Figure 3 The Chinese patent CN 114537005A will not be described in detail here.

[0172] The appearance, OD density, film thickness μm, surface impedance, and pull-out of the prepared black photoresist composition coatings 1-12 were tested. The test results are shown in Table 2. The test method is as follows:

[0173] The appearance of the black photoresist coating is determined by visual inspection.

[0174] OD density: Under normal temperature and pressure conditions, the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested using an optical densitometer LS117 at 5 points on each sample, and the ink thickness was <15 μm.

[0175] Film thickness: Use a step film thickness meter (Japanese small board ET200A-3D step meter) or a probe film thickness meter.

[0176] Surface impedance: Under normal temperature and pressure conditions, the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested for the resistivity of the ink at 5 points using an impedance meter ACL-800.

[0177] Pull-off: The test was conducted using the OU4080 pull-off adhesion tester.

[0178] Table 2:

[0179] Surface gloss OD density Film thickness um Surface impedance Pull-out force N / m Example 1 Black 6 4.1 10x10E11 45 Example 2 Black 6 4.4 10x10E11 42 Example 3 Black 5.2 4.8 10x10E11 46 Example 4 Black 5.6 4.2 10x10E11 48 Example 5 Black 4.9 4.6 10x10E11 44 Example 6 Black 4.9 4.6 10x10E11 44 Example 7 Black 5.2 4.3 10x10E11 48 Example 8 Black 5.3 5.5 10x10E11 50 Example 9 Black 5.4 4.4 10x10E11 44 Example 10 Black 5.1 4.6 10x10E11 44 Embodiment 11 Black 5.0 6.0 10x10E11 55 Example 12 Black 4.9 5.5 10x10E11 52 Comparative Example 1 gray 2.3 11.7 10x10E8 25 Comparative Example 2 Ash 1.4 16.2 10x10E8 25

[0180] The obtained black photoresist composition coatings 1 to 12 were subjected to resistivity, dyne value, OD, hundred grid test, surface hardness, boiling test, alcohol resistance test, alkali resistance test, acid resistance test, high temperature and high humidity test, high temperature test, and low temperature test. The test results are shown in Table 3. The test method is as follows:

[0181] Surface impedance: Under normal temperature and pressure conditions, the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested for the resistivity of the ink at 5 points using an impedance meter ACL-800.

[0182] Dyne value: Under normal temperature and pressure conditions, the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested using a dyne pen. The cap of the dyne pen was removed, the pen face was placed in parallel contact with the screen printing surface, a 5 cm long line was appropriately drawn on the ink surface, and a stopwatch was turned on for 2 seconds before observation.

[0183] OD density: Under normal temperature and pressure conditions, the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested using an optical densitometer LS117 at 5 points on each sample, and the ink thickness was <15 μm.

[0184] Grid test: Under normal temperature and pressure conditions, for the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12, make the grid knife form an angle of 15° to 30° with the glass film layer in the selected test area, use enough force to make the knife tip contact the glass film layer, move the grid knife close to the glass surface to cross-draw lines on the glass film layer, clean the surface of the glass film layer with a brush, and rub it with fingers to make sure there are no bubbles or wrinkles between the tape and the film layer. However, do not use too much force, wait for 90±30 seconds, slowly tear off the tape at an angle of 180°, and then observe the peeling.

[0185] Surface hardness: The pencil method was used to test the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12. A pencil with a hardness of 3H and a load of 500 g was used to scratch the black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 at a test angle of 45° at different positions with 5 strokes, each stroke being 7 mm long. The scratches were observed.

[0186] Boiling test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested in a water bath, placed in a constant temperature water bath at 100° C., and boiled for 1 hour. After the test was completed, a hundred-grid test was performed to observe the shedding.

[0187] Alcohol resistance test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were tested 50 times with a dust-free cloth dipped in alcohol and loaded with 1000 g by the wear tester to observe the shedding.

[0188] Alkali resistance test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were dotted on the ink surface using 5% NaOH solution, and the appearance was observed after standing for 24 hours, and a cross-sectional test was performed, and then the shedding was observed.

[0189] Acid resistance test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were dotted on the ink surface with 5% H2SO4 solution, and the appearance was observed after standing for 24 hours, and a cross-sectional test was performed, and then the shedding was observed.

[0190] High temperature and high humidity test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were affixed with structural adhesive and some structural parts, and then placed in a constant temperature and humidity test box at 85°C / 85%RH for 1000 hrs. After being taken out and restored to room temperature for 2 hours, the test was performed.

[0191] High temperature test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were affixed with structural adhesive and some structural parts, and then placed in a 90°C constant temperature test box for 1000 hrs. After being taken out and restored to room temperature for 2 hrs, the test was performed.

[0192] Low temperature test: The black photoresist composition coatings 1 to 12 obtained in Examples 1 to 12 were affixed with structural adhesive and some structural parts, and then placed in a -40°C constant temperature test box for 1000 hrs. After being taken out and restored to room temperature for 2 hrs, the test was performed.

[0193] Table 3:

[0194]

[0195] See also Figure 4 and Figure 5 , Figure 4 and Figure 5 The black photoresist composition coatings prepared in Example 1 and Example 2 are respectively developed in 0.045% KOH solution. It can be seen that the black frame prepared by the black photoresist composition of the present invention is clear and has no residue.

[0196] See also Figure 7 , Figure 7 The black film layer is the finished product prepared in Example 2 without the auxiliary agent A. Figure 7 In the figure, the white part in the upper right corner is due to the lack of additive A, which causes the black film layer to be uneven. Due to the lack of additive A in Example 2, the black photoresist prepared in Example A has poor leveling properties, resulting in the black film layer having a partially uneven black film layer.

[0197] See also Figure 8 , Figure 8 The black film layer is the finished product prepared in Example 3 without the auxiliary agent B. Figure 8 In the figure, the white part is the area where the film surface falls off after the weather resistance test is performed on the black film surface prepared in Example 3. Due to the lack of the auxiliary agent B in Example 3, the adhesion of the black film surface prepared in Example 3 is weakened, and it performs poorly in the weather resistance test.

[0198] See also Fig. 9 , Fig. 9 The middle black film layer is the finished product prepared by adding additives A and B in Example 1. Fig. 9 The white area in the middle is the blank area after development. It can be seen that after the photolithography process, there is no burr or "sawtooth" on the vertical edge of the developed area. Moreover, after the photoresist film is formed and cured, the surface is glossy and black, the leveling is normal, and there is no edge return on the surrounding borders.

[0199] This is because during the post-lithography curing process, the additive A can significantly change the surface tension, viscosity, and leveling of the photoresist solvent system, improving the construction properties of the spray coating. Moreover, under the action of the photoinitiator, a fluorine group is introduced during the polymerization process, similar to the following structure. A small amount of fluorine-containing polymerized structure can improve the weather resistance of the light-shielding film layer formed after the black photoresist is cured.

[0200] The auxiliary agent B can undergo a Cope elimination reaction with the β-H atom tertiary amine resin to participate in photopolymerization curing. The resin containing unsaturated bonds obtained by the Cope elimination reaction of the β-H atom tertiary amine resin can also be polymerized with the remaining unreacted photocurable resin monomer to increase the crosslinking density. The use of the auxiliary agent B can improve the adhesion of the black photoresist film surface of the present invention and enhance the weather resistance of the black photoresist of the present invention.

[0201] Combined with the results in the above table, it can be seen that the black frame of the black photoresist after film formation and curing is resistant to acid, alkali, solvent, stripping liquid, and copper etching liquid; it is resistant to metal plating at 25-280℃; in a high temperature and high humidity environment of 85℃ / 85%, the square resistance is stable at 5.0×10 12 The photoresist of the present invention has the advantages of more than 100 ohms / □. After the film is formed and cured, the surface is glossy and black, and the OD density, film thickness, surface impedance and pull-out resistance are far superior to the black frame obtained by UV inkjet process and pad printing process, and the dosage can be reduced in production process applications. As in Example 1 and Comparative Example 2, under the condition of achieving the same shading effect, the film thickness of the black frame obtained by the present invention is one-fourth of that of the UV inkjet process. After the photolithography process, the minimum development accuracy can reach 3μm, and the black frame is made without burrs or "sawtooths".

[0202] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A black photoresist composition, characterized in that: The photoresist composition comprises an alkali-soluble photopolymer resin, a photocurable resin monomer, an auxiliary agent A, an auxiliary agent B, a photoinitiator, a thermal initiator, a black colorant, and a polar organic solvent; Among them, the photopolymer resin includes two types of resins: bisphenol fluorene acrylic resin and tertiary amine resin containing β-H atoms; In parts by weight, the black photoresist composition includes 2 to 20 parts of the bisphenol fluorene acrylic resin, 1 to 10 parts of the tertiary amine resin containing β-H atoms, 0.1 to 2 parts of auxiliary agent A, 0.2 to 5 parts of auxiliary agent B, 0.5 to 2 parts of the photoinitiator, 5 to 10 parts of the photocurable resin monomer, 10 to 50 parts of the black colorant and 50 to 500 parts of the polar organic solvent.

2. The black photoresist composition according to claim 1, wherein The bisphenol fluorene acrylic resin is selected from one or more compounds shown in general formula (I); wherein n is an integer of 10 to 180; R1 and R3 are CH2; R2 and R4 are OH; X and W are A is selected from H or C1-2 alkyl.

3. The black photoresist composition according to claim 1, characterized in that The mass ratio of the bisphenol fluorene acrylic resin to the tertiary amine resin containing β-H atoms is in the range of 1:1 to 5:1, and the tertiary amine resin containing β-H atoms is selected from one or more compounds shown in general formula (II); Among them, R is A is selected from H or C1-2 alkyl; R1 is selected from -H, -CH3, R2 is selected from phenyl, benzyl, phenol.

4. The black photoresist composition according to claim 1, characterized in that The photoinitiator is a carbazole oxime ester compound, and the photoinitiator is selected from one or more compounds shown in general formula (III); Wherein R1 is selected from R2 is selected from R3 is selected from , R4 is selected from 5. The black photoresist composition according to claim 1, wherein The photocurable resin monomer is an acrylic resin, and the photocurable resin monomer is selected from one or more compounds shown in general formula (IV) and (V); R1 is selected from and R2 is selected from -H and The mass ratio of the photoinitiator to the photocurable resin monomer is in the range of 1:100 to 2:

5.

6. The black photoresist composition according to claim 1, characterized in that The polar organic solvent is an organic non-protonic polar solvent with medium polarity and strong polarity, selected from ethylene glycol ethyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, triethoxy methacrylate, acetone, butanone, cyclohexanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate or one or more, and the mass ratio of the polar organic solvent to the photocurable resin monomer is between 5:1 and 100:1, preferably between 10:1 and 80:1, and more preferably between 20:1 and 70:

1.

7. The black photoresist composition according to claim 1, wherein The black colorant is selected from one or more of cyanine black, aniline black, carbon black, titanium black, and graphite black. The black colorant is preferably carbon black particles. The size of the carbon black particles is 100nm to 200nm, and the mass ratio of the carbon black particles to the photocurable resin monomer is in the range of 10:1 to 1:

1.

8. The black photoresist composition according to claim 1, wherein The auxiliary agent A contains a perfluorinated substituted vinyl monomer, and the perfluorinated substituted vinyl monomer is selected from the compounds shown in the general formula (VI); Wherein, R1, R2, R3, R4 are selected from One of them.

9. The black photoresist composition according to claim 1, characterized in that: The auxiliary agent B comprises at least one aromatic peroxide, and can undergo Cope elimination reaction with the β-H atom tertiary amine resin during post-photolithography curing to participate in photopolymerization curing, and the aromatic peroxide is selected from the compounds shown in general formula (VII); Wherein, R5 is selected from one of -F, -Cl and -Br.

10. The black photoresist composition according to claim 1, wherein The thermal initiator comprises a bisimidazole compound, and the bisimidazole compound is selected from the compounds shown in general formula (VIII); Wherein, R1 and R2 are independently selected from -H, methyl or ethyl.

11. A method for preparing a black photoresist composition according to any one of claims 1 to 10, characterized in that: The preparation method comprises the following steps: (1) preparing a black color paste: adding an organic solvent to a sand mill with zirconium balls of 0.05-0.1 mm in size to wet-grind the black colorant, and adding the bisphenol fluorene acrylic resin composition as a stabilizing resin during the grinding process to prepare a black color paste; (2) preparing a photosensitive solution: mixing and dispersing the tertiary amine resin containing β-H atoms, the photocurable resin, the photoinitiator, the auxiliary agent A, the auxiliary agent B, and the polar organic solvent according to the formula amount into a solution and filtering the solution to obtain a photosensitive solution; (3) Preparing a black photoresist composition: mixing the black color paste in step (1) and the photosensitive solution in step (2), and finally adding an organic solvent to adjust the viscosity, dispersing the mixture in a disperser to form a uniform solution, and filtering the mixture to obtain a black photoresist composition.

12. A process for manufacturing a black frame of a curved display glass base cover, characterized in that: The following steps are involved: S11: spraying a first layer of black photoresist as described in any one of claims 1 to 12 on the heat-bent curved glass substrate in the x direction by inkjet process, and pre-baking to form a black photoresist film with a thickness of 1-3 μm; S12: using LDI laser direct writing lithography to partially expose the frame pattern, and after washing away the black photoresist in the frame through a developing process, the first layer of black frame is formed after post-baking and hardening; S13: spraying a second layer of the black photoresist according to any one of claims 1 to 12 in the y direction on the curved substrate with the first black border by inkjet technology, and pre-baking to form a second layer of black photoresist film with a thickness of 1-3 μm; S14: using LDI laser direct writing lithography again to partially expose the frame pattern, and after washing away the black photoresist in the frame through a development process, a second layer of black frame is formed after post-baking and hardening; The post-baking temperature in S12 and S14 is 200-250°C.

Citation Information

Patent Citations

  • High-temperature-resistant epoxy resin and preparation method thereof

    CN110066382A

  • Curved window glass transfer printing process

    CN114537005A

Cited By

  • Black photoresist composition and use method thereof

    CN119535893A

  • Black photoresist composition and preparation method therefor, and black bezel manufacturing process

    WO2025218679A1