Silver paste for ultrahigh-voltage annular zinc oxide varistor and preparation method of silver paste

By increasing the use of inorganic adhesives and sheet powder, combined with the introduction of boron oxide and bismuth oxide, the welding resistance problem of the annular zinc oxide varistor at high voltage and high temperature is solved, and the welding resistance of the cyclic zinc oxide varistor is achieved at high voltage and high temperature. The product stability and solderability are improved, meeting the needs of high-end electronic products.

CN119049757APending Publication Date: 2024-11-29HEFEI SHENGDA ELECTRONIC TECH IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107234.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing annular zinc oxide varistor products are prone to silver consumption under high voltage and high temperature welding conditions, resulting in unqualified products and difficult to meet the high voltage needs of high-end products such as new energy vehicles and home appliances.

Method used

By increasing the amount of inorganic adhesive and introducing flake powder, the bulk density of silver powder is improved, the sintering performance of silver particles is improved, and boron oxide and bismuth oxide are introduced into the inorganic adhesive to form a complex to reduce the melting point and Viscosity ensures that the inorganic binder softens and flows into the substrate before the silver layer is densified, avoiding surface cracking and degradation of welding.

Benefits of technology

The high voltage of the annular zinc oxide pressure-sensitive product reaches 120V, improves welding resistance and welding temperature to 360℃, reduces welding silver corrosion, reduces the unqualified rate, and maintains the surface quality and welding properties of the product. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049757A_ABST
    Figure CN119049757A_ABST
Patent Text Reader

Abstract

The invention relates to silver paste for an ultrahigh-voltage annular zinc oxide varistor and a preparation method of the silver paste, and the silver paste for the ultrahigh-voltage annular zinc oxide varistor is prepared from the following components in percentage by mass: 45-55 wt% of sphere-like silver powder, 20-30 wt% of superfine spherical silver powder, 0.5 wt% of flake silver powder and 10-20 wt% of an organic carrier, and 3 to 15 wt% of an inorganic binder. The annular zinc oxide voltage-sensitive product can have high voltage by increasing the addition amount of the inorganic adhesive in the silver paste, and the problems of product surface cracking, bubbling, weldability reduction and the like are avoided by adding a small amount of flake silver powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic pastes, and in particular to a silver paste for an ultra-high voltage annular zinc oxide varistor and a preparation method thereof. Background Art

[0002] Zinc oxide varistor is a common nonlinear overvoltage protection semiconductor component. It utilizes the nonlinear characteristics of zinc oxide varistor. When the voltage applied to the varistor is lower than its threshold, the current flowing through it is extremely small, and it is equivalent to an infinite resistance and is in an off state; when the voltage applied to the varistor exceeds its threshold, the current flowing through it surges to protect electrical appliances. It is often used in the commutator part of the motor to reduce brush sparks, electromagnetic interference and noise, and extend the life of electrical appliances. Therefore, it is widely used in various electronic products such as new energy vehicles, home appliances, computers, industrial protection, and military electronic products.

[0003] At present, most of the electronic silver pastes used in the annular varistor industry are produced from spherical ultrafine silver powders. The average particle size of the silver powders is generally 0.5-1.2 μm, and the specific surface area is 3.0-6.0 m 2 / g. The silver paste prepared by this type of silver powder is tested for welding under the condition of keeping the silver content and printing thickness the same. The silver surface can withstand a low welding temperature (the industry currently generally uses 220-230℃ for spot welding). When the temperature exceeds 230℃ and the welding time exceeds 2s, silver is easily eaten away, resulting in unqualified products.

[0004] With the development of information technology, high voltage requirements have been put forward for annular zinc oxide varistors. Currently, the voltage of annular zinc oxide varistors on the market is generally 3-80V, and there are only a small number of 80-100V products. It is increasingly difficult to meet the needs of new energy vehicles, home appliances, and high-end computer products. Therefore, it is particularly important to develop silver paste for annular zinc oxide varistors that exceed the voltage. Summary of the invention

[0005] Based on this, the purpose of the present invention is to provide a silver paste for an ultra-high voltage annular zinc oxide varistor and a preparation method thereof. In order to increase the voltage of the annular zinc oxide varistor product, the silver paste for the ultra-high voltage annular zinc oxide varistor increases the amount of inorganic adhesive added in the silver paste, so that the annular zinc oxide varistor product can reach an astonishing 120V. At the same time, in order to avoid problems such as cracking, blistering and decreased solderability of the product surface, a small amount of flaky powder is introduced to increase the packing density of the silver powder, making it easier for the silver particles to sinter together, thereby improving the solder resistance.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention provides a silver paste for an ultra-high voltage annular zinc oxide varistor, which is prepared from the following components in percentage by mass: 45-55wt% of quasi-spherical silver powder, 20-30wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 10-20wt% of an organic carrier, and 3-15wt% of an inorganic binder.

[0008] The present invention can make the annular zinc oxide varistor product have a high voltage of up to an astonishing 120V by increasing the addition amount of the inorganic adhesive. At the same time, by adding a small amount of flaky silver powder, the packing density of the silver powder is increased, so that the silver particles are more easily sintered together, thereby improving the soldering resistance. At the same time, the flaky silver powder can reduce the sintering activity of the slurry, so that the inorganic adhesive softens and flows into between the silver layer and the matrix. At the same time, the flaky silver powder has a large specific surface area and a small lattice gap after sintering, and it is not easy for the inorganic adhesive to float, thereby avoiding problems such as cracking, blistering and decreased solderability of the product surface. The present invention also adds quasi-spherical silver powder to directly improve the soldering resistance, increase the previous welding temperature from 230°C to 360°C, increase the soldering resistance time by 1-2 seconds, effectively prevent the phenomenon of silver corrosion during welding, and reduce the unqualified rate.

[0009] As a further improvement of the above solution of the present invention, the particle diameter of the spherical silver powder is 3-6 μm, and the specific surface area is 3.2 m 2 / g;

[0010] And / or, the particle diameter of the ultrafine spherical silver powder is 400-800nm, and the specific surface area is 7.0m 2 / g;

[0011] And / or, the length of the flaky silver powder is 10-12 μm. The present invention selects flaky silver powder with a suitable length of 10-12 μm, which can reduce the sintering activity of the slurry, soften the inorganic binder and flow into the space between the silver layer and the matrix. At the same time, the flaky silver powder has a large specific surface area and a small lattice gap after sintering, which makes it difficult for the inorganic binder to float.

[0012] As a further improvement of the above solution of the present invention, the inorganic binder is BaO, CaO, Bi 2 O 3 , ZnO, CuO, B 2 O 3 、SiO 2At least one of the following. The boron oxide and bismuth oxide introduced in the present invention in the non-polar bonding, the boric acid molecule contains three hydroxyl groups, which can form a complex with the metal oxide in the process of forming the inorganic binder, thereby reducing the melting point and viscosity, so that the inorganic binder can be softened before the silver layer is densified; the bismuth oxide is easy to combine with the bismuth oxide in the porcelain body to provide good adhesion, and the bismuth oxide has a high specific gravity, which can be increased to the density of glass, so that the density of the inorganic binder is greater than that of silver, so that it can flow smoothly between the silver layer and the substrate, so that the prepared silver paste has a high voltage, and at the same time avoids the problems of sintering cracking, blistering and reduced solderability.

[0013] As a further improvement of the above solution of the present invention, the inorganic binder is prepared from the following components in percentage by weight: 3-5wt% BaO, 0-5wt% CaO, 50-85wt% Bi 2 O 3 , 3-5wt% ZnO, 1-15wt% CuO, 5-17wt% B 2 O 3 , 2-8wt% SiO 2 .

[0014] As a further improvement of the above scheme of the present invention, the preparation method of the inorganic binder is: weigh BaO, CaO, Bi 2 O 3 , ZnO, CuO, B 2 O 3 、SiO 2 After mixing evenly, pour into a crucible, put into a 1100-1300°C martensite furnace and keep warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind with agate balls, and dry to obtain an inorganic binder with a particle size of ≤10μm.

[0015] As a further improvement of the above scheme of the present invention, the organic carrier comprises an organic solvent, an organic additive and a polymer thickener, the content of the organic solvent is 7-13wt% of the total amount of silver paste for the ultra-high voltage annular zinc oxide varistor, the content of the organic additive is 0-1wt% of the total amount of silver paste for the ultra-high voltage annular zinc oxide varistor, and the content of the polymer thickener is 3-6wt% of the total amount of silver paste for the ultra-high voltage annular zinc oxide varistor.

[0016] As a further improvement of the above scheme of the present invention, the preparation method of the organic carrier is: mix the polymer thickener and the organic solvent in proportion and heat to 70-140°C, and continue stirring until the polymer thickener is completely dissolved; then add the organic auxiliary agent in proportion, stir, and cool to room temperature to obtain the organic carrier.

[0017] As a further improvement of the above solution of the present invention, the organic solvent is at least one of terpineol, tributyl citrate and a film-forming aid;

[0018] As a further improvement of the above solution of the present invention, the organic auxiliary agent is at least one of dispersant BYK111, dispersant BYK333, and dispersant S007;

[0019] And / or, the polymer thickener is ethyl cellulose.

[0020] The present invention provides a method for preparing a silver paste for an ultra-high voltage annular zinc oxide varistor as described above, comprising the following steps: weighing quasi-spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier, and inorganic binder in proportion and mixing them evenly, and then grinding until a slurry with a particle size of ≤10 μm and uniform dispersion is obtained.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] In order to improve the voltage of the annular zinc oxide varistor product, the present invention increases the amount of inorganic binder added in the silver paste, so that the annular zinc oxide varistor product has a high voltage, reaching an astonishing 120V; at the same time, in order to avoid problems such as cracking, blistering and decreased solderability of the product surface: on the one hand, by adding a small amount of flaky silver powder, the packing density of the silver powder is increased, so that the silver particles are more easily sintered together, thereby improving the solder resistance, and at the same time, the flaky silver powder can reduce the sintering activity of the slurry, so that the inorganic binder softens and flows into between the silver layer and the matrix, and at the same time, the flaky silver powder has a large specific surface area and a small lattice gap after sintering and forming, and it is not easy for the inorganic binder to float, thereby avoiding cracking on the product surface. On the other hand, the boron oxide and bismuth oxide introduced in the non-polar bonding of the present invention contain three hydroxyl groups in the boric acid molecule, which can form a complex with the metal oxide in the process of forming the inorganic binder, thereby reducing the melting point and viscosity, so that the inorganic binder can be softened before the silver layer is densified, and the bismuth oxide is easy to combine with the bismuth oxide in the matrix to provide good adhesion. At the same time, the specific gravity of bismuth oxide can be increased to the density of glass, so that the density of the inorganic binder is greater than that of silver, so that it can flow smoothly between the silver layer and the matrix. Through the above two points, the material of the present invention can have a high voltage under high non-polar bonding conditions, while avoiding the problems of sintering cracking, blistering and reduced solderability.

[0023] The present invention also adds spherical silver powder to directly improve the soldering resistance, raising the previous soldering temperature from 230°C to 360°C, increasing the soldering time by 1-2 seconds, effectively preventing the phenomenon of silver corrosion during soldering and reducing the unqualified rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a 1000 times SEM crystal growth image of the silver paste for the ultra-high voltage annular zinc oxide varistor prepared in Example 1;

[0025] Figure 2 This is a 1000x SEM crystal growth image of the silver paste for the ultra-high voltage annular zinc oxide varistor prepared in Comparative Example 1;

[0026] Figure 3 This is a microscope photo of a ring-shaped zinc oxide varistor prepared using the silver paste prepared in Example 3;

[0027] Figure 4 This is a microscope photograph of a ring-shaped zinc oxide varistor prepared using the silver paste prepared in Comparative Example 3. DETAILED DESCRIPTION

[0028] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0030] Example 1

[0031] The present embodiment provides a silver paste for an ultra-high voltage annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 46wt% of quasi-spherical silver powder, 30wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 4wt% of inorganic binder, 10wt% of pine alcohol, 3wt% of tributyl citrate, 6wt% of ethyl cellulose, and 0.5wt% of dispersant BYK111.

[0032] 100g of inorganic binder includes: 5% BaO, 5% CaO, 55% Bi 2 O 3 , 5% ZnO, 5% CuO, 17% B 2 O 3 , 8% SiO 2The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0033] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0034] S1. Weigh each raw material according to the proportion;

[0035] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol and tributyl citrate are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant BYK111 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0036] S3. Preparation of slurry: After fully mixing the quasi-spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier and inorganic binder, use a three-roll mill to roll until a slurry with a particle size of ≤10μm and uniform dispersion is obtained, that is, the silver paste for ultra-high voltage annular zinc oxide varistor is obtained. The silver paste prepared in this embodiment has a viscosity of 100-250Pa·S, 25°C; the sintering temperature is 750-850°C.

[0037] Example 2

[0038] This embodiment provides a silver paste for an ultra-high voltage annular zinc oxide varistor, which includes the following raw materials by weight: 55wt% of quasi-spherical silver powder, 20wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 9wt% of inorganic binder, 7wt% of pine alcohol, 3wt% of film-forming aid, 4.5wt% of ethyl cellulose, and 1wt% of dispersant S007;

[0039] In this embodiment, 100g of the inorganic binder includes: 3% BaO, 85% Bi 2 O 3 , 4% ZnO, 1% CuO, 5% B 2 O 3 , 2%SiO 2The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0040] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0041] S1. Weigh each raw material according to the proportion;

[0042] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol and film-forming aid are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant S007 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0043] S3. Preparation of slurry: After fully mixing the quasi-spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier and inorganic binder, use a three-roll mill to roll until a slurry with a particle size of ≤10μm and uniform dispersion is obtained, that is, the silver paste for ultra-high voltage annular zinc oxide varistor is obtained. The silver paste prepared in this embodiment has a viscosity of 100-250Pa·S, 25°C; the sintering temperature is 750-850°C.

[0044] Example 3

[0045] The present embodiment provides a silver paste for an ultra-high voltage annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 50wt% of quasi-spherical silver powder, 20wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 12wt% of inorganic binder, 10wt% of pine alcohol, 1wt% of tributyl citrate, 6wt% of ethyl cellulose, and 0.5wt% of dispersant BYK333.

[0046] In this embodiment, 100g of the inorganic binder includes: 4% BaO, 3% CaO, 59% Bi 2 O 3 , 4% ZnO, 15% CuO, 10% B 2 O 3 , 5%SiO 2The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0047] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0048] S1. Weigh each raw material according to the proportion;

[0049] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol and tributyl citrate are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant BYK333 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0050] S3. Preparation of slurry: After fully mixing the quasi-spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier and inorganic binder, use a three-roll mill to roll until a slurry with a particle size of ≤10μm and uniform dispersion is obtained, that is, the silver paste for ultra-high voltage annular zinc oxide varistor is obtained. The silver paste prepared in this embodiment has a viscosity of 100-250Pa·S, 25°C; the sintering temperature is 750-850°C.

[0051] Example 4

[0052] The present embodiment provides a silver paste for an ultra-high voltage annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 47wt% of spherical silver powder, 30wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 5wt% of inorganic binder, 10.5wt% of pine alcohol, 2.5wt% of film-forming aid, 3.5wt% of ethyl cellulose, and 1wt% of dispersant S007.

[0053] In this embodiment, 100g of the inorganic binder includes: 3% BaO, 4% CaO, 63% Bi 2 O 3 , 3% ZnO, 10% CuO, 15% B 2 O 3 , 2%SiO 2The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0054] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0055] S1. Weigh each raw material according to the proportion;

[0056] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol and film-forming aid are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant S007 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0057] S3. Preparation of slurry: After fully mixing the quasi-spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier and inorganic binder, use a three-roll mill to roll until a slurry with a particle size of ≤10μm and uniform dispersion is obtained, that is, the silver paste for ultra-high voltage annular zinc oxide varistor is obtained. The silver paste prepared in this embodiment has a viscosity of 100-250Pa·S, 25°C; the sintering temperature is 750-850°C.

[0058] Comparative Example 1

[0059] This comparative example proposes a silver paste for annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 47wt% of quasi-spherical silver powder, 30wt% of ultrafine spherical silver powder, 5wt% of inorganic binder, 10wt% of pine alcohol, 3wt% of tributyl citrate, 4wt% of ethyl cellulose, and 1wt% of dispersant BYK111.

[0060] In this embodiment, 100g of inorganic binder includes: 5% BaO, 5% CaO, 10% Bi 2 O 3 , 5% ZnO, 5% CuO, 5% B 2 O 3 , 5%SiO 2 , 60%P 2 O 3The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0061] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0062] S1. Weigh each raw material according to the proportion;

[0063] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol and tributyl citrate are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant BYK111 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0064] S3. Preparation of slurry: After fully stirring and mixing the quasi-spherical silver powder, ultrafine spherical silver powder, organic carrier and inorganic binder, the mixture is rolled with a three-roll mill until a slurry with a particle size of ≤10 μm and uniform dispersion is obtained, that is, a silver paste for ultra-high voltage annular zinc oxide varistor is obtained.

[0065] Comparative Example 2

[0066] This comparative example proposes a silver paste for annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 50wt% of spherical silver powder, 28wt% of ultrafine spherical silver powder, 8wt% of inorganic binder, 5wt% of pine alcohol, 3wt% of tributyl citrate, 2wt% of film-forming aid, 3wt% of ethyl cellulose, and 1wt% of dispersant BYK333.

[0067] In this embodiment, 100g of inorganic binder includes: 5% BaO, 5% CaO, 10% Bi 2 O 3 , 5% ZnO, 5% CuO, 5% B 2 O 3 , 5%SiO 2 , 60%P 2 O 3The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0068] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0069] S1. Weigh each raw material according to the proportion;

[0070] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol, tributyl citrate and film-forming aid are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant BYK333 is added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0071] S3. Preparation of slurry: After fully stirring and mixing the quasi-spherical silver powder, ultrafine spherical silver powder, organic carrier and inorganic binder, the mixture is rolled with a three-roll mill until a slurry with a particle size of ≤10 μm and uniform dispersion is obtained, that is, a silver paste for ultra-high voltage annular zinc oxide varistor is obtained.

[0072] Comparative Example 3

[0073] This comparative example proposes a silver paste for annular zinc oxide varistor, which includes the following component raw materials in percentage by mass: 50wt% of spherical silver powder, 20wt% of ultrafine spherical silver powder, 12wt% of inorganic binder, 10wt% of pine alcohol, 1wt% of tributyl citrate, 2wt% of film-forming aid, 4wt% of ethyl cellulose, 0.5wt% of dispersant BYK111, and 0.5wt% of dispersant BYK333.

[0074] In this embodiment, 100g of inorganic binder includes: 5% BaO, 5% CaO, 10% Bi 2 O 3 , 5% ZnO, 5% CuO, 5% B 2 O 3 , 5%SiO 2 , 60%P 2 O 3The preparation process of the inorganic binder is as follows: weigh each component in proportion and mix them mechanically with a high-efficiency mixer for 30 minutes, put them into a muffle furnace at 1100-1300°C and keep them warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind them with agate balls for 50 hours until the powder particle size is ≤10μm, and dry them at 120°C to obtain the inorganic binder.

[0075] The method for preparing the silver paste for the ultra-high voltage annular zinc oxide varistor of this embodiment comprises the following steps:

[0076] S1. Weigh each raw material according to the proportion;

[0077] S2. Preparation of organic carrier: ethyl cellulose, pinene alcohol, tributyl citrate and film-forming aid are stirred and mixed, and the mixture is stirred at 70-140°C for 1.5-2.5h (stirring speed is 40-130RPM) to completely dissolve the ethyl cellulose, and finally dispersant BYK111 and dispersant BYK333 are added to the above mixed system, stirred for 1.5-2.5h and cooled to room temperature to obtain an organic carrier.

[0078] S3. Preparation of slurry: After fully stirring and mixing the quasi-spherical silver powder, ultrafine spherical silver powder, organic carrier and inorganic binder, the mixture is rolled with a three-roll mill until a slurry with a particle size of ≤10 μm and uniform dispersion is obtained, that is, a silver paste for ultra-high voltage annular zinc oxide varistor is obtained.

[0079] The proportions of the above embodiments and comparative examples are shown in Table 1.

[0080] Table 1 Proportions of Examples and Comparative Examples (mass percentage)

[0081] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Spherical silver powder 46 55 50 47 47 50 50 Ultrafine spherical silver powder 30 20 20 30 30 28 20 Flake silver powder 0.5 0.5 0.5 0.5 0 0 0 Inorganic adhesive 4 9 12 5 5 8 12 Terpineol 10 7 10 10.5 10 5 10 Tributyl citrate 3 0 1 0 3 3 1 Film-forming aids 0 3 0 2.5 0 2 2 Ethyl cellulose 6 4.5 6 3.5 4 3 4 BYK111 0.5 0 0 0 1 0 0.5 BYK333 0 0 0.5 0 0 1 0.5 S007 0 1 0 1 0 0 0

[0082] Figure 1 , Figure 2 The crystal growth images of the silver paste for the annular zinc oxide varistor prepared in Example 1 and Comparative Example 1 at 1000 times SEM. Figure 1 It can be seen that the size of the silver crystals in Example 1 is about 18-25 μm, which is much larger than the size of the silver crystals in Comparative Example 1. This is crucial to the solder resistance of the product and the electrical properties after welding. Per unit area, the larger the crystal, the smaller the lattice gap, and the solder is difficult to corrode the silver layer, which can effectively reduce the voltage drop of the product. At the same time, larger crystals can also improve the conductivity of the product.

[0083] Test Case

[0084] The silver paste for the annular zinc oxide varistor prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-3 was used to prepare annular zinc oxide varistor samples and 30 samples were prepared respectively. The preparation process of the annular zinc oxide varistor samples was as follows: the prepared silver paste was printed on annular zinc oxide ceramic sheets by an automatic printing machine, and then the obtained product was dried at 150°C. After drying, the annular zinc oxide varistor product was obtained by sintering at 850°C for 1 hour.

[0085] Figure 3 , Figure 4 The following are microscope photos of the annular zinc oxide varistors prepared using the silver pastes prepared in Example 3 and Comparative Example 3, respectively. Figure 3 It can be seen that Example 3 did not have blistering or cracking at a high inorganic binder addition amount, and the surface sintering effect was good. This is because the inorganic binder in this example has the following two characteristics: 1. a low softening point, and 2. a high density, so that it can penetrate into the space between the substrate and the silver layer before the silver layer is densified, thereby avoiding a decrease in the solderability of the product. Figure 4 It can be seen that in comparative example 3, when the amount of inorganic binder added is high, a large number of bubbles will appear in the traditional silver paste, and even cracks will occur during sintering. This shows that the slurry prepared by the present invention breaks through the amount of inorganic binder added in the traditional slurry while maintaining a good sintering state.

[0086] The prepared annular zinc oxide varistor was installed on a DC motor and used to test the performance of the prepared annular zinc oxide varistor. The test results are shown in Table 2. However, in the process of preparing annular zinc oxide varistor samples using the silver paste of the annular zinc oxide varistor prepared in Comparative Example 3, bubbling and cracking occurred, so it was a defective product and could not be tested.

[0087] Table 2

[0088]

[0089] Note: The resistor size is 9.4mm in outer diameter and 5.7mm in inner diameter; E10 and E1 are the voltage values ​​when the current is 10mA and 1mA respectively; R10 and R1 are the percentages of the three-pole difference of E10 and E1 respectively ((maximum voltage value - minimum voltage value) / minimum voltage value).

[0090] It can be seen from the results in Table 2 that: the three-pole difference of the embodiment of the present application is smaller than that of the comparative example, which means that the consistency of the slurry in the embodiment of the present application and the ohmic contact between the slurry and the porcelain body are better than those of the comparative example; and the higher nonlinear coefficient also means that the embodiment has a better ability to absorb surge current; the voltage drop of the embodiment after welding is smaller than that of the comparative example, indicating that the resistance to solder corrosion of the embodiment is better than that of the comparative example; the tensile force of the embodiment is greater than that of the comparative example, proving that the embodiment is in closer contact with the porcelain body and the metallization layer is not easy to fall off; the firing voltage range of the embodiment is also wider than that of the comparative example, which can meet the needs of different customers.

[0091] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A silver paste for ultra-high voltage annular zinc oxide varistor, It is characterized in that The invention is prepared from the following components in percentage by mass: 45-55wt% of quasi-spherical silver powder, 20-30wt% of ultrafine spherical silver powder, 0.5wt% of flaky silver powder, 10-20wt% of organic carrier and 3-15wt% of inorganic binder.

2. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 1, It is characterized in that The particle diameter of the spherical silver powder is 3-6 μm, and the specific surface area is 3.2 m 2 / g; the particle diameter of the ultrafine spherical silver powder is 400-800nm ​​and the specific surface area is 7.0m 2 / g; the length of the flaky silver powder is 10-12 μm.

3. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 1, It is characterized in that The inorganic binder is BaO, CaO, Bi 2 O 3 , ZnO, CuO, B 2 O 3 、SiO 2 At least one of .

4. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 3, It is characterized in that The inorganic binder is prepared from the following components in percentage by weight: 3-5wt% BaO, 0-5wt% CaO, 50-85wt% Bi 2 O 3 , 3-5wt% ZnO, 1-15wt% CuO, 5-17wt% B 2 O 3 , 2-8wt% SiO 2 .

5. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 4, It is characterized in that The preparation method of the inorganic binder is: weigh BaO, CaO, Bi in proportion 2 O 3 , ZnO, CuO, B 2 O 3 、SiO 2 After mixing evenly, pour into a crucible, put into a 1100-1300°C martensite furnace and keep warm for 10-15 minutes to obtain a molten mixture; then pour the molten mixture into cold water to form granular glass crystals, grind with agate balls, and dry to obtain an inorganic binder with a particle size of ≤10μm.

6. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 1, It is characterized in that The organic carrier comprises an organic solvent, an organic auxiliary agent and a polymer thickener, wherein the content of the organic solvent is 7-13wt% of the total amount of the silver paste for the ultra-high voltage annular zinc oxide varistor, the content of the organic auxiliary agent is 0-1wt% of the total amount of the silver paste for the ultra-high voltage annular zinc oxide varistor, and the content of the polymer thickener is 3-6wt% of the total amount of the silver paste for the ultra-high voltage annular zinc oxide varistor.

7. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 5, It is characterized in that The preparation method of the organic carrier is: a polymer thickener and an organic solvent are mixed in proportion and heated to 70-140° C., and stirred continuously until the polymer thickener is completely dissolved; then an organic auxiliary agent is added in proportion, stirred, and cooled to room temperature to obtain the organic carrier.

8. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 6, It is characterized in that The organic solvent is at least one of terpineol, tributyl citrate and a film-forming aid.

9. The silver paste for ultra-high voltage annular zinc oxide varistor according to claim 6, It is characterized in that The organic additive is at least one of dispersant BYK111, dispersant BYK333, and dispersant S007; And / or, the polymer thickener is ethyl cellulose.

10. A method for preparing a silver paste for an ultra-high voltage annular zinc oxide varistor according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Spherical silver powder, ultrafine spherical silver powder, flaky silver powder, organic carrier and inorganic binder are weighed in proportion and mixed evenly, and then ground until a slurry with a particle size of ≤10 μm and uniform dispersion is obtained.