Heavy rare earth segregation type temperature-resistant high-performance neodymium iron boron permanent magnet and preparation method thereof

By adding aluminum, nickel and Mg nanopowder to the NdFeB permanent magnet and adopting a semi-polymerized structure of heavy rare earth elements, the problem of degradation of magnetic properties of NdFeB permanent magnet at high temperatures is solved, and its high temperature resistance is significantly improved Performance and magnetic properties enhance the resistance to demagnetization and corrosion resistance.

CN119049862AActive Publication Date: 2024-11-29JIANGSU CHANNELON ELECTRONIC GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411251051.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing neodymium iron boron permanent magnets have reduced magnetic properties at high temperatures, and their corrosion resistance and coercivity are insufficient. The existing technology has failed to effectively improve their temperature resistance and magnetic properties.

Method used

By adding aluminum, nickel and Mg nanopowder to the NdFeB permanent magnet and adopting a semi-polymerized structure of heavy rare earth elements, it is formed by vacuum smelting, hydrogen breaking, airflow grinding, orientation pressing and sintering, and other processes, and is formed with high density and NdFeB permanent magnet with excellent magnetic properties.

Benefits of technology

It significantly improves the high temperature resistance, magnetic properties and thermal stability of NdFeB permanent magnets, enhances its anti-magnetization ability and coercivity, and improves corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032262200000131
    Figure BDA0005032262200000131
  • Figure BDA0005032262200000141
    Figure BDA0005032262200000141
Patent Text Reader

Abstract

The invention discloses a heavy rare earth segregation type temperature-resistant high-performance neodymium iron boron permanent magnet and a preparation method thereof. The specific preparation method comprises the following steps: S1, weighing a main alloy raw material and an auxiliary alloy raw material according to a certain proportion; s2, the weighed main alloy raw materials and the weighed auxiliary alloy raw materials are subjected to vacuum melting, hydrogen demolishing and airflow grinding treatment correspondingly, and main phase magnetic powder and auxiliary phase powder are prepared; s3, mixing the main-phase magnetic powder with the auxiliary-phase powder, and carrying out orientation compression molding treatment on the mixed material to obtain a magnet green body; and S4, sintering and tempering the magnet green body, and cooling to obtain the neodymium-iron-boron permanent magnet with the heavy rare earth segregation type structure. The high temperature resistance of the magnet can be improved by adding aluminum and nickel elements, the Curie temperature can be increased and the temperature coefficient can be reduced by adding a proper amount of cobalt element, so that the heat resistance of the neodymium-iron-boron permanent magnet is improved, and the magnetic performance and the temperature resistance of the neodymium-iron-boron permanent magnet are further improved by adding Mg nano powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of NdFeB permanent magnets, in particular to a method for preparing a heavy rare earth segregated type heat-resistant and high-performance NdFeB permanent magnet. Background Art

[0002] NdFeB permanent magnets are tetragonal magnetic materials formed by neodymium, iron and boron. NdFeB permanent magnets have extremely high magnetic energy product and coercive force. At the same time, the advantages of high energy density make NdFeB permanent magnet materials widely used in modern industry and electronic technology.

[0003] The NdFeB permanent magnets in the prior art have strong magnetic properties at room temperature, but their magnetic properties decrease as the temperature rises. Therefore, when preparing the NdFeB permanent magnets, their temperature resistance needs to be considered.

[0004] The defects of existing NdFeB permanent magnets are:

[0005] 1. In the preparation process of existing NdFeB permanent magnets, little consideration is given to improving the high temperature resistance of NdFeB, which makes the thermal stability of NdFeB permanent magnets excellent;

[0006] 2. Patent document CN105489368B proposes a method for preparing NdFeB permanent magnets. However, the method for preparing NdFeB in the patent document does not consider improving the corrosion resistance and magnetic properties of NdFeB permanent magnets by increasing the density and orientation of the magnets.

[0007] 3. In the prior art, the magnetic properties of NdFeB permanent magnets prepared according to conventional NdFeB permanent magnet preparation methods are already excellent, so there is little consideration of further improving the magnetic properties of NdFeB permanent magnets;

[0008] 4. Patent document CN104966607B discloses a method for preparing sintered NdFeB permanent magnets. For the magnets in this patent document in which the heavy rare earth elements are only concentrated on the surface of the grains, if the strength of the external magnetic field is large enough, once the magnetic domain wall breaks through the high anisotropy layer on the surface, the magnetic domains in the low anisotropy field region inside the grains will instantly reverse magnetization, and the final coercive force of the magnet will also be relatively low. Summary of the invention

[0009] The object of the present invention is to provide a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0010] To achieve the above object, the present invention provides the following technical solution: a method for preparing a heavy rare earth segregated heat-resistant and high-performance neodymium iron boron permanent magnet, comprising the following steps:

[0011] S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio;

[0012] S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen cracking and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder;

[0013] S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body;

[0014] S4, sintering and tempering the magnet green body, and cooling to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure;

[0015] Wherein, in S1, the main alloy raw materials include 32 to 36 parts of neodymium powder, 62 to 70 parts of iron powder, 4.8 to 4.9 parts of boron powder, 0.04 to 0.07 parts of copper powder, 0.3 to 0.8 parts of aluminum powder, 0.4 to 0.7 parts of nickel powder and 0.6 to 0.8 parts of cobalt powder in parts by weight;

[0016] In S3, during the mixing process of the main phase magnetic powder and the auxiliary phase powder, 0.08 wt% to 0.12 wt% of Mg nanopowder is added.

[0017] Preferably, in S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 6 to 13 parts of gadolinium, 13 to 14 parts of terbium, 8 to 15 parts of aluminum powder and 15 to 19 parts of copper powder.

[0018] Preferably, in the vacuum smelting step of S2, the smelting temperature of the smelting furnace is 1400°C to 1600°C, and the smelting holding time is 25min to 65min.

[0019] Preferably, in the hydrogen cracking step of S2, the smelted material is fed into a hydrogen cracking furnace, evacuated to a vacuum degree of less than or equal to 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa~2×10 5 Pa, the hydrogen cracking treatment time is 3.8h~4.5h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

[0020] Preferably, in the air flow milling step of S2, the material after hydrogen rupture is collected and sent to an air flow mill for air flow milling to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 2.6 μm to 3.2 μm.

[0021] Preferably, in the orientation pressing step of S3, the pressing step adopts a combined pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 2.5T~4.2T, the molding pressure is 15Mpa~55Mpa, the isostatic pressing pressure is 180Mpa~250Mpa, and the holding time is 30s~150s.

[0022] Preferably, in the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours, the magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours, and then cooled in the furnace to obtain a sintered body.

[0023] Preferably, in the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment;

[0024] Primary tempering treatment: tempering temperature 850℃~1200℃, time 1.5h~8h;

[0025] Secondary tempering treatment: tempering temperature 450℃~800℃, time is 1.5h~6h.

[0026] Preferably, a heavy rare earth segregated type heat-resistant and high-performance NdFeB permanent magnet is provided, wherein the NdFeB permanent magnet is divided into a main phase and an auxiliary phase, wherein the main phase is an alloy containing NdFeB; the auxiliary phase is an alloy of heavy rare earths, and the main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth elements diffuse into the main phase grains to form a segregation layer and a heavy rare earth surface layer.

[0027] Preferably, the segregation layer is located inside the heavy rare earth surface layer, and the concentration of heavy rare earth elements is higher than that of the heavy rare earth surface layer. The thickness of the segregation layer is 0.2 μm to 3 μm, and the thickness of the heavy rare earth surface layer is 1 μm to 5 μm.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention can improve the high temperature resistance of the magnet by adding aluminum and nickel elements. The addition of cobalt can not only increase the Curie temperature, but also reduce the temperature coefficient, thereby improving the heat resistance of the NdFeB permanent magnet. By adding an appropriate amount of cobalt element and adding Mg nanopowder, the temperature resistance of the permanent magnet can be improved while ensuring the excellent magnetic properties of the magnet.

[0030] 2. The present invention can significantly improve the magnetic properties and thermal stability of NdFeB magnets by adding Mg nanopowder. This improvement is mainly achieved through the distribution of Mg nanopowder in the grain boundary area, which improves the wettability of the neodymium-rich phase along the main phase particles, improves the microstructure of the grain boundary phase, and refines the main phase grains, thereby improving the magnetic properties of the magnet and improving the thermal stability of the NdFeB permanent magnet. The addition of an appropriate amount of Mg nanopowder can make the density of the magnet reach the maximum value and improve the orientation of the magnet, thereby helping to improve the corrosion resistance of the permanent magnet.

[0031] 3. The present invention improves the temperature resistance of the NdFeB permanent magnet by adding appropriate amounts of aluminum and nickel to the NdFeB permanent magnet. At the same time, the addition of cobalt can also increase the coercive force and magnetic saturation of the NdFeB permanent magnet. The introduction of the auxiliary alloy makes the main phase grains chemically heterogeneous, further enhancing the magnetic properties of the magnet.

[0032] 4. The present invention mixes the main alloy and the auxiliary alloy to diffuse the heavy rare earth elements into the main phase grains to form a segregation layer and a heavy rare earth surface layer, so that the main phase grains of the NdFeB permanent magnet have a heavy rare earth segregation structure. The magnet with the grains of this structure can prevent the reverse magnetization domain from moving into the interior of the magnet, thereby improving the anti-demagnetization ability and coercive force of the magnet. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] An embodiment provided by the present invention is a method for preparing a heavy rare earth segregated heat-resistant and high-performance neodymium iron boron permanent magnet, comprising the following steps:

[0035] S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio;

[0036] S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen cracking and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder;

[0037] S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body;

[0038] S4, sintering and tempering the magnet green body, and cooling to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure;

[0039] Wherein, in S1, the main alloy raw materials include 32 to 36 parts of neodymium powder, 62 to 70 parts of iron powder, 4.8 to 4.9 parts of boron powder, 0.04 to 0.07 parts of copper powder, 0.3 to 0.8 parts of aluminum powder, 0.4 to 0.7 parts of nickel powder and 0.6 to 0.8 parts of cobalt powder in parts by weight;

[0040] In S3, during the mixing process of the main phase magnetic powder and the auxiliary phase powder, 0.08 wt% to 0.12 wt% of Mg nanopowder is added.

[0041] In S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 6 to 13 parts of gadolinium, 13 to 14 parts of terbium, 8 to 15 parts of aluminum powder and 15 to 19 parts of copper powder.

[0042] In the vacuum melting step of S2, the melting temperature of the melting furnace is 1400°C to 1600°C, and the melting and holding time is 25min to 65min.

[0043] In the hydrogen crushing step of S2, the smelted material is sent to the hydrogen crushing furnace, evacuated to a vacuum degree less than or equal to 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa~2×10 5 Pa, the hydrogen cracking treatment time is 3.8h~4.5h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

[0044] In the air flow grinding step of S2, the materials after hydrogen crushing are collected and sent to an air flow grinder for air flow grinding to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 2.6 μm to 3.2 μm.

[0045] In the orientation pressing step of S3, the pressing step adopts a combined pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 2.5T~4.2T, the molding pressure is 15Mpa~55Mpa, the isostatic pressing pressure is 180Mpa~250Mpa, and the holding time is 30s~150s.

[0046] In the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours. The magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours. The green body is cooled in the furnace to obtain a sintered body.

[0047] In the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment;

[0048] Primary tempering treatment: tempering temperature 850℃~1200℃, time 1.5h~8h;

[0049] Secondary tempering treatment: tempering temperature 450℃~800℃, time 1.5h~6h;

[0050] A heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet is prepared according to the above-mentioned method for preparing a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet. The NdFeB permanent magnet is divided into a main phase and an auxiliary phase, wherein the main phase is an alloy containing NdFeB; the auxiliary phase is an alloy of heavy rare earths, and the main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth elements diffuse into the main phase grains to form a segregation layer and a heavy rare earth surface layer, the segregation layer is located on the inner side of the heavy rare earth surface layer, and the concentration of the heavy rare earth elements is higher than that of the heavy rare earth surface layer, the thickness of the segregation layer is 0.2μm to 3μm, and the thickness of the heavy rare earth surface layer is 1μm to 5μm.

[0051] Furthermore, in the preparation process of NdFeB permanent magnets, neodymium is one of the main rare earth metal elements of NdFeB permanent magnets, and is one of the key elements to improve the coercive force and remanence of NdFeB permanent magnets. Iron is one of the main reference elements of NdFeB permanent magnets and is one of the most important components of alloy materials. Boron is one of the important components to improve the coercive force and magnetic saturation of NdFeB permanent magnets.

[0052] Nickel can improve the corrosion resistance of the permanent magnet. Aluminum is one of the necessary elements to increase the oxidation resistance and high temperature resistance of NdFeB permanent magnets. The high temperature resistance of the magnet can be improved by adding aluminum, nickel and other elements. Copper is one of the necessary elements to increase the electrical conductivity of NdFeB permanent magnets. Cobalt is one of the important components to increase the coercive force and magnetic saturation of NdFeB permanent magnets. Adding cobalt to NdFeB permanent magnets can significantly improve the temperature resistance. The addition of cobalt can not only increase the Curie temperature, but also reduce the temperature coefficient, thereby improving the heat resistance of NdFeB alloys.

[0053] The introduction of auxiliary alloy makes the main phase grains chemically heterogeneous, further enhancing the magnetic properties of the magnet; the NdFeB rare earth permanent magnet has a heavy rare earth element segregation structure in the main phase grains, the heavy rare earth element surface concentration in the main phase grains of the magnet is low, and the internal segregation layer concentration is high. The magnet with grains of this structure can prevent the reverse magnetization domain from moving into the interior of the magnet, thereby improving the magnet's anti-demagnetization ability and coercive force.

[0054] By adding Mg nanopowder, the magnetic properties and thermal stability of NdFeB magnets can be significantly improved. This improvement is mainly achieved by the distribution of Mg nanopowder in the grain boundary area, which improves the wettability of the Nd-rich phase along the main phase particles, improves the microstructure of the grain boundary phase, and refines the main phase grains, thereby improving the magnetic properties of the magnet. The addition of Mg nanopowder also improves the thermal stability of NdFeB permanent magnets. At high temperatures, NdFeB permanent magnets are prone to aging, resulting in reduced magnetic properties. However, by adding Mg nanopowder, this performance degradation trend can be slowed down to a certain extent. Especially when the temperature does not exceed 100°C, after adding an appropriate amount of Mg nanopowder, the remanence, coercive force and maximum magnetic energy product of the NdFeB permanent magnet have basically the same downward trend with the increase of temperature, indicating that Mg nanopowder has a certain effect on improving thermal stability. Adding Mg nanopowder to NdFeB permanent magnets can change the microstructure of the grain boundary and the magnet density, thereby achieving the improvement of the magnetic properties of the NdFeB permanent magnets.

[0055] The addition of Mg nanopowder to permanent magnets can increase the corrosion potential of permanent magnets, reduce the corrosion current density and increase the charge migration resistance, thereby improving the corrosion resistance of permanent magnets. By adding an appropriate amount of Mg nanopowder, the density of the magnet can be maximized and the orientation of the magnet can be improved, all of which help to improve corrosion resistance.

[0056] In the preparation process of the NdFeB permanent magnet of the present invention, the main component ratios of neodymium, iron and boron are relatively reasonable, and other trace elements and rare earth elements that can promote the performance and temperature resistance of the magnet are added to ensure that the performance of the prepared permanent magnet is better. At the same time, the molding method is reasonable.

[0057] Embodiment 1:

[0058] An embodiment provided by the present invention is a method for preparing a heavy rare earth segregated heat-resistant and high-performance neodymium iron boron permanent magnet, comprising the following steps:

[0059] S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio;

[0060] S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen cracking and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder;

[0061] S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body;

[0062] S4, sintering and tempering the magnet green body, and cooling to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure;

[0063] Wherein, in S1, the main alloy raw materials include 33 parts of neodymium powder, 65 parts of iron powder, 4.85 parts of boron powder, 0.05 parts of copper powder, 0.5 parts of aluminum powder, 0.5 parts of nickel powder and 0.7 parts of cobalt powder in parts by weight;

[0064] In S3, 0.1 wt% of Mg nanopowder is added during the mixing process of the main phase magnetic powder and the auxiliary phase powder.

[0065] In S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 9 parts of gadolinium, 13 parts of terbium, 10 parts of aluminum powder and 15 parts of copper powder.

[0066] In the vacuum melting step of S2, the melting temperature of the melting furnace is 1500°C, and the melting holding time is 40 minutes.

[0067] In the hydrogen crushing step of S2, the smelted material is sent to the hydrogen crushing furnace, evacuated to a vacuum degree of less than 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa, the hydrogen cracking treatment time is 4.5h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

[0068] In the air flow milling step of S2, the materials after hydrogen crushing are collected and sent to an air flow mill for air flow milling to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 2.6 μm.

[0069] In the orientation pressing step of S3, the pressing step adopts a combination pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 3.2T, the molding pressure is 45Mpa, the isostatic pressing pressure is 200Mpa, and the holding time is 100s.

[0070] In the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours. The magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours. The green body is cooled in the furnace to obtain a sintered body.

[0071] In the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment;

[0072] First-stage tempering treatment: tempering temperature 1000℃, time 4h;

[0073] Secondary tempering treatment: tempering temperature 600℃, time 4h;

[0074] A heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet is prepared according to the above-mentioned method for preparing a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet. The NdFeB permanent magnet is divided into a main phase and an auxiliary phase, the main phase is an alloy containing NdFeB; the auxiliary phase is an alloy of heavy rare earth, and the main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth element diffuses into the main phase grains to form a segregation layer and a heavy rare earth surface layer, the segregation layer is located on the inner side of the heavy rare earth surface layer, and the concentration of the heavy rare earth element is higher than that of the heavy rare earth surface layer, the thickness of the segregation layer is 0.4μm, and the thickness of the heavy rare earth surface layer is 1μm.

[0075] Embodiment 2:

[0076] An embodiment provided by the present invention is a method for preparing a heavy rare earth segregated heat-resistant and high-performance neodymium iron boron permanent magnet, comprising the following steps:

[0077] S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio;

[0078] S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen cracking and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder;

[0079] S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body;

[0080] S4, sintering and tempering the magnet green body, and cooling to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure;

[0081] Among them, in S1, the main alloy raw materials include 34 parts of neodymium powder, 67 parts of iron powder, 4.8 parts of boron powder, 0.06 parts of copper powder, 0.4 parts of aluminum powder, 0.6 parts of nickel powder and 0.68 parts of cobalt powder in parts by weight;

[0082] In S3, 0.09 wt% of Mg nanopowder is added during the mixing process of the main phase magnetic powder and the auxiliary phase powder.

[0083] In S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 10 parts of gadolinium, 13 parts of terbium, 12 parts of aluminum powder and 15 parts of copper powder.

[0084] In the vacuum melting step of S2, the melting temperature of the melting furnace is 1500°C, and the melting holding time is 55 minutes.

[0085] In the hydrogen crushing step of S2, the smelted material is sent to the hydrogen crushing furnace, evacuated to a vacuum degree of 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa, the hydrogen cracking treatment time is 4h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

[0086] In the air flow milling step of S2, the materials after hydrogen crushing are collected and sent to an air flow mill for air flow milling to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 3.2 μm.

[0087] In the orientation pressing step of S3, the pressing step adopts a combination pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 4T, the molding pressure is 35Mpa, the isostatic pressing pressure is 220Mpa, and the holding time is 110s.

[0088] In the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours. The magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours. The green body is cooled in the furnace to obtain a sintered body.

[0089] In the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment;

[0090] First-stage tempering treatment: tempering temperature 1200℃, time 2h;

[0091] Secondary tempering treatment: tempering temperature 800℃, time 1.5h;

[0092] A heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet is prepared according to the above-mentioned method for preparing a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet. The NdFeB permanent magnet is divided into a main phase and an auxiliary phase, the main phase is an alloy containing NdFeB; the auxiliary phase is an alloy of heavy rare earth, and the main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth element diffuses into the main phase grains to form a segregation layer and a heavy rare earth surface layer, the segregation layer is located on the inner side of the heavy rare earth surface layer, and the concentration of the heavy rare earth element is higher than that of the heavy rare earth surface layer, the thickness of the segregation layer is 0.3μm, and the thickness of the heavy rare earth surface layer is 1.2μm.

[0093] Embodiment three:

[0094] An embodiment provided by the present invention is a method for preparing a heavy rare earth segregated heat-resistant and high-performance neodymium iron boron permanent magnet, comprising the following steps:

[0095] S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio;

[0096] S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen cracking and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder;

[0097] S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body;

[0098] S4, sintering and tempering the magnet green body, and cooling to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure;

[0099] Wherein, in S1, the main alloy raw materials include 36 parts of neodymium powder, 70 parts of iron powder, 4.9 parts of boron powder, 0.07 parts of copper powder, 0.8 parts of aluminum powder, 0.7 parts of nickel powder and 0.8 parts of cobalt powder in parts by weight;

[0100] In S3, 0.11 wt% of Mg nanopowder is added during the mixing process of the main phase magnetic powder and the auxiliary phase powder.

[0101] In S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 13 parts of gadolinium, 14 parts of terbium, 15 parts of aluminum powder and 15 parts of copper powder.

[0102] In the vacuum melting step of S2, the melting temperature of the melting furnace is 1450°C, and the melting holding time is 35 minutes.

[0103] In the hydrogen crushing step of S2, the smelted material is sent to the hydrogen crushing furnace, evacuated to a vacuum degree less than or equal to 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa, the hydrogen cracking treatment time is 3.8h~4.5h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

[0104] In the air flow milling step of S2, the materials after hydrogen crushing are collected and sent to an air flow mill for air flow milling to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 2.6 μm.

[0105] In the orientation pressing step of S3, the pressing step adopts a combination pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 3.5T, the molding pressure is 35Mpa, the isostatic pressing pressure is 180Mpa, and the holding time is 150s.

[0106] In the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours. The magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours. The green body is cooled in the furnace to obtain a sintered body.

[0107] In the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment;

[0108] First-stage tempering treatment: tempering temperature 1000℃, time 6h;

[0109] Secondary tempering treatment: tempering temperature 500℃, time 6h;

[0110] A heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet is prepared according to the above-mentioned method for preparing a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet. The NdFeB permanent magnet is divided into a main phase and an auxiliary phase, the main phase is an alloy containing NdFeB; the auxiliary phase is an alloy of heavy rare earth, and the main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth element diffuses into the main phase grains to form a segregation layer and a heavy rare earth surface layer, the segregation layer is located on the inner side of the heavy rare earth surface layer, and the concentration of the heavy rare earth element is higher than that of the heavy rare earth surface layer, the thickness of the segregation layer is 2μm, and the thickness of the heavy rare earth surface layer is 4μm.

[0111] Comparative Example 1:

[0112] The preparation method of this comparative example is different from that of Example 1 in that, in S3, during the mixing process of the main phase magnetic powder and the auxiliary phase powder, no Mg nanopowder is added, and the rest is the same as that of Example 1.

[0113] Comparative Example 2:

[0114] This comparative example provides a method for preparing a NdFeB permanent magnet, and the specific steps are as follows:

[0115] S1. Preprocessing

[0116] Weigh the raw materials in proportion and perform vacuum melting to obtain NdFeB ingots;

[0117] S2, Hydrogen Fragmentation

[0118] The NdFeB ingot is subjected to hydrogen explosion treatment to obtain NdFeB particles;

[0119] S3, Flour Milling

[0120] Grinding the NdFeB particles to obtain NdFeB powder;

[0121] S4, Forming

[0122] The NdFeB powder is pressed and molded, and the pressing conditions are as follows: an oriented pressing magnetic field of 2T, an isostatic pressure of 250MPa, and a pressing time of 90s to obtain a NdFeB blank;

[0123] S5. Sintering

[0124] The NdFeB blank is subjected to vacuum sintering and secondary tempering treatment. The vacuum sintering includes two stages:

[0125] In the first stage, the temperature is first heated to 760°C at room temperature and kept for 1 hour at a heating rate of 7°C / min. In the second stage, the temperature is raised to 1020°C and kept for 1.5 hours at a heating rate of 5°C / min, and then naturally cooled to obtain NdFeB permanent magnets.

[0126] The raw materials of the NdFeB permanent magnet of this comparative example include the following components by weight:

[0127] 138 parts of praseodymium and neodymium, 20 parts of holmium iron, 40 parts of cerium, 30 parts of boron, 1.2 parts of copper, 3 parts of aluminum, 4 parts of zirconium, 3 parts of cobalt, and 385 parts of iron.

[0128] The NdFeB permanent magnet prepared by the preparation method of this comparative example does not have grains with a heavy rare earth segregation structure.

[0129] The weight ratio of raw materials and Mg nanopowder added in the above examples and comparative examples is as follows:

[0130]

[0131] According to the GB / T3217 permanent magnet material magnetic test method, the magnetic properties of the NdFeB permanent magnets obtained in Examples 1-3 and Comparative Examples 1-2 were tested. The test results are shown in Table:

[0132]

[0133] Combined with the above implementation and comparative examples, and combined with the test results for analysis:

[0134] By comparing Examples 1-3 with Comparative Examples 1-2, the NdFeB permanent magnets prepared by the preparation method of the present invention have excellent magnetic properties, and the magnets with heavy rare earth segregated structural grains can prevent the movement of the reverse magnetization domains into the interior of the magnet, thereby improving the anti-demagnetization ability and coercive force of the magnets, and adding Mg nanopowder to the NdFeB permanent magnets can change the microstructure of the grain boundaries and the magnet density, thereby achieving the improvement of the magnetic properties of the NdFeB permanent magnets.

[0135] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a heavy rare earth segregated heat-resistant high-performance neodymium iron boron permanent magnet, comprising the following steps: S1. Weigh the main alloy raw material and the auxiliary alloy raw material according to a certain ratio; S2, weighing the main alloy raw material and the auxiliary alloy raw material and performing vacuum melting, hydrogen crushing and air flow grinding treatment respectively to prepare the main phase magnetic powder and the auxiliary phase powder; S3, mixing the main phase magnetic powder with the auxiliary phase powder, and performing orientation pressing and molding on the mixed material to obtain a magnet green body; S4, sintering and tempering the magnet green body, and cooling it to obtain a NdFeB permanent magnet with a heavy rare earth segregation structure; in, In S1, the main alloy raw materials include 32 to 36 parts of neodymium powder, 62 to 70 parts of iron powder, 4.8 to 4.9 parts of boron powder, 0.04 to 0.07 parts of copper powder, 0.3 to 0.8 parts of aluminum powder, 0.4 to 0.7 parts of nickel powder and 0.6 to 0.8 parts of cobalt powder in parts by weight; In S3, during the mixing process of the main phase magnetic powder and the auxiliary phase powder, 0.08 wt% to 0.12 wt% of Mg nanopowder is added.

2. A method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In S1, the auxiliary alloy is an alloy of heavy rare earths, and the raw materials of the auxiliary alloy include 6 to 13 parts of gadolinium, 13 to 14 parts of terbium, 8 to 15 parts of aluminum powder and 15 to 19 parts of copper powder.

3. A method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the vacuum melting step of S2, the melting temperature of the melting furnace is 1400°C to 1600°C, and the melting and holding time is 25min to 65min.

4. The method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the hydrogen crushing step of S2, the smelted material is sent to the hydrogen crushing furnace, evacuated to a vacuum degree less than or equal to 3.2 Pa, and hydrogen is introduced to maintain the pressure at 1.6×10 5 Pa~2×10 5 Pa, the hydrogen cracking treatment time is 3.8h~4.5h. After the residual hydrogen is extracted, the hydrogen cracking furnace is heated to 460℃ and kept warm for 3.6h.

5. The method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the air flow grinding step of S2, the materials after hydrogen crushing are collected and sent to an air flow grinder for air flow grinding to obtain main phase magnetic powder and auxiliary phase powder with a particle size of 2.6 μm to 3.2 μm.

6. The method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the orientation pressing step of S3, the pressing step adopts a combined pressing method of vertical pressing and isostatic pressing, the orientation magnetic field is 2.5T~4.2T, the molding pressure is 15Mpa~55Mpa, the isostatic pressing pressure is 180Mpa~250Mpa, and the holding time is 30s~150s.

7. The method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the sintering step of S4, the magnet green body is heated to 800° C. in a vacuum furnace and sintered for 2 hours. The magnet green body is further heated to 1150° C. in a vacuum furnace and sintered for 3.5 hours. The green body is cooled in the furnace to obtain a sintered body.

8. The method for preparing a heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 1, Features: In the tempering step of S4, the tempering treatment adopts a two-stage tempering treatment; Primary tempering treatment: tempering temperature 850℃~1200℃, time 1.5h~8h; Secondary tempering treatment: tempering temperature 450℃~800℃, time is 1.5h~6h.

9. A heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet, prepared according to the method for preparing a heavy rare earth segregated heat-resistant high-performance NdFeB permanent magnet according to claim 1, It is characterized in that The NdFeB permanent magnet is divided into a main phase and an auxiliary phase, wherein the main phase is an alloy containing NdFeB; The auxiliary phase is an alloy of heavy rare earths. The main phase grains of the NdFeB permanent magnet have a heavy rare earth element segregation structure, wherein the heavy rare earth elements diffuse into the main phase grains to form a segregation layer and a heavy rare earth surface layer.

10. A heavy rare earth segregated heat-resistant and high-performance NdFeB permanent magnet according to claim 9, Features: The segregation layer is located inside the heavy rare earth surface layer, and the concentration of heavy rare earth elements is higher than that of the heavy rare earth surface layer. The thickness of the segregation layer is 0.2 μm to 3 μm, and the thickness of the heavy rare earth surface layer is 1 μm to 5 μm.

Citation Information

Patent Citations

  • Rare earth permanent magnet produced by using abundant rare earth La and preparation method thereof

    CN103093912A

  • Dual-alloy neodymium-iron-boron rare earth permanent magnet and manufacturing method thereof

    CN108015293A

  • High-coercivity sintered neodymium-iron-boron magnet and preparation method thereof

    CN113838622A

  • Neodymium-iron-boron rare earth permanent magnet with heavy rare earth element segregation structure in crystal grains and preparation method and application thereof

    CN117059357A

  • Graphene-Containing Rare Earth Permanent Magnet Material And Preparation Method Thereof

    US20220301752A1