High-conductivity nano-porous nickel-nickel oxide loaded silver nanoflower electrode material and preparation method and application thereof
By introducing silver nanoflower structures into nanoporous nickel-nickel oxide electrode materials and combining dealloying and electrochemical activation techniques, the problems of poor conductivity and easy agglomeration were solved, and the preparation of nanoporous nickel-nickel oxide electrode materials with high conductivity and high specific capacitance was realized, which are suitable for supercapacitors.
Patent Information
- Application Number
- CN202411384299.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing nanoporous nickel-nickel oxide electrode materials have poor conductivity, are prone to agglomeration, have complicated and costly preparation processes, are difficult to mass-produce, and do not have outstanding electrochemical performance.
A composite structure consisting of a silver-nickel-based amorphous alloy as the middle core layer, nanoporous nickel-nickel oxide layers on both sides, and silver nanoflowers on the outermost layer was prepared by dealloying and electrochemical activation methods to produce highly conductive nanoporous nickel-nickel oxide-supported silver nanoflower materials.
It improves the conductivity and interfacial wettability of electrode materials, increases the surface area, and significantly enhances rate performance and specific capacitance. The preparation process is simple, safe, and low-cost, making it suitable for large-scale production.
Smart Images

Figure CN119049888A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of capacitor electrode materials, and in particular relates to a highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material, and a preparation method and application thereof. Background Art
[0002] With the growth of the world's population and the rapid development of the economy, energy and environmental issues are increasingly becoming the core of mankind's sustainable development strategy. Due to the non-renewable nature of fossil fuels and the instability of renewable energy sources such as wind and solar energy, it is urgent to develop new energy storage devices that are cleaner, more environmentally friendly, stable and long-lasting. Supercapacitors are widely used in transportation, aerospace, mobile communications and other fields because of their energy density close to that of batteries, fast charging and discharging performance, safety and environmental protection, etc., attracting the research interest of scientific researchers from all over the world.
[0003] Transition metal oxide - NiO has high theoretical specific capacity and high cycle stability, and is low-priced and abundant in resources. It is expected to become a new generation of high-quality supercapacitor electrode materials. Nickel oxide has a variety of crystal forms and valences. During the charge and discharge process, it undergoes a reversible redox reaction accompanied by the conversion between different valences to produce pseudocapacitors. The specific capacity and stored energy produced are much higher than those of carbon-based electrode materials based on electrolyte ion adsorption and desorption. However, as a semiconductor material, bulk NiO has poor conductivity and low utilization of internal NiO, which seriously limits the rate performance and specific capacitance of the electrode. Therefore, the development of nano-sized NiO and the improvement of its conductivity have become the focus of research.
[0004] The Chinese patent application document with publication number CN102874884A discloses a method for preparing nickel oxide, a supercapacitor electrode material. In the patent, porous flower-shaped nickel oxide is prepared by mixing nickel nitrate hexahydrate, polyvinyl pyrrolidone, formaldehyde and water, and the mixed solution is injected into a hydrothermal reactor after stirring evenly. The hydrothermal reaction is carried out at 150-200°C for 3-24 hours, and then the supercapacitor electrode material is obtained by cooling, centrifugation, drying and calcination. The porous flower-shaped NiO electrode material prepared by this method has both high specific capacitance and good electrochemical stability, but the NiO material is a powdered electrode material, and the nano-powdered electrode material is easy to agglomerate during use, resulting in a decrease in electrode performance; the preparation process is cumbersome, high temperature and high pressure, and the cost is high, and its industrialization degree is low. At the same time, the patent only provides a method for preparing NiO, which cannot be directly applied to supercapacitors. It needs to be mixed with a conductive agent and an adhesive to form a slurry and coated on a conductive substrate to form an electrode.
[0005] The Chinese patent application document with publication number CN107240507A discloses a nanoporous nickel-nickel oxide supercapacitor electrode material and its preparation method. In the patent, a self-supporting nanoporous nickel-nickel oxide supercapacitor electrode material is prepared by a three-step method of "dealloying-oxidation immersion-heat treatment". The electrode is a layered structure, namely a rod-shaped nickel oxide layer, a nanoporous layer, and an intermediate amorphous core layer. The nanoporous layer and the intermediate amorphous core layer of the electrode have no active substances and only play a current collecting role. The electroactive substance is the rod-shaped nickel oxide on the surface of the electrode. The conductivity of the single nickel oxide is poor, so its electrochemical performance is not outstanding. In addition, the preparation process is relatively complicated, with many steps, and is not suitable for large-scale production. Summary of the invention
[0006] The technical problem to be solved by the present invention is how to provide a highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower material and a preparation method thereof.
[0007] The present invention solves the above technical problems through the following technical means:
[0008] The first aspect of the present invention provides a nanoporous nickel-nickel oxide loaded silver nanoflower material, which is composed of a silver-containing nickel-based amorphous alloy, a nanoporous nickel-nickel oxide layer and silver nanoflowers; the silver-containing nickel-based amorphous alloy is used as an intermediate core layer, and nanoporous nickel-nickel oxide layers are arranged on both sides of the intermediate core layer, and the outermost layer is silver nanoflowers; the silver nanoflowers are composed of silver nanosheets or silver nanoparticles, which are uniformly distributed on the surface of the nanoporous nickel-nickel oxide; the composition of the silver-containing nickel-based amorphous alloy is Ni 40-x (Zr,Ti) 60 Ag x , where the subscripts are the atomic percentages of the elements, 5≤x≤10.
[0009] Preferably, the thickness ratio of the silver-containing nickel-based amorphous alloy core layer, the nanoporous nickel-nickel oxide layer, and the silver nanoflowers is 2:1 to 3:1.
[0010] Preferably, the diameter of the silver nanoflower is 0.5-3 μm, the size of the silver nanosheet is 0.2-1.5 μm, and the diameter of the silver nanoparticle is 0.1-0.5 μm.
[0011] Preferably, the composition of the silver-containing nickel-based amorphous alloy is Ni 30 Zr 60 Ag 10 、Ni 30 Ti 60 Ag 10 or Ni 30 Zr 20 Ti 40 Ag 10 .
[0012] The second aspect of the present invention provides a method for preparing the above-mentioned highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower material, comprising the following steps:
[0013] (1) Preparation of Ni-Zr / Ti-Ag or Ni-Zr-Ti-Ag amorphous alloy strips:
[0014] According to the composition of the silver-containing nickel-based amorphous alloy, Ni, Zr / Ti, Ag or Ni, Zr, Ti, Ag are mixed, and the mixed alloy raw materials are evenly melted to obtain a Ni-Zr / Ti-Ag or Ni-Zr-Ti-Ag alloy ingot; the obtained alloy ingot is heated to a molten state, and the alloy liquid is blown out by an inert gas, so that the molten liquid metal solidifies on a rotating copper roller to obtain a silver-containing nickel-based amorphous alloy strip;
[0015] (2) Dealloying to prepare supersaturated nanoporous nickel-silver alloy:
[0016] placing a silver-containing nickel-based amorphous alloy strip in an acid solution, then taking it out and washing it to obtain a supersaturated nanoporous nickel-silver alloy;
[0017] (3) Preparation of nanoporous nickel-nickel oxide-loaded silver nanoflowers by electrochemical activation:
[0018] The supersaturated nanoporous nickel-silver alloy is placed in an alkaline solution and electrochemically activated by cyclic voltammetry (CV) to obtain a nanoporous nickel-nickel oxide-loaded silver nanoflower material.
[0019] Preferably, the purity of Ni, Ti, Zr and Ag is 99.9wt.%.
[0020] Preferably, the rotation speed of the copper roller is 34-36 m / s.
[0021] Preferably, the silver-containing nickel-based amorphous alloy strip has a thickness of 20 to 50 μm and a width of 1.5 to 2 cm.
[0022] Preferably, the acid solution is a mixture of H3PO4 and NH3F, wherein the concentration of NH3F is 0.02-0.5M, the concentration of H3PO4 is 0.02-0.5M; and the molar ratio of H3PO4 to NH3F is 1:1.
[0023] Preferably, the alkaline solution is a NaOH or KOH solution with a concentration of 1 to 6M.
[0024] Preferably, the potential window of the cyclic voltammetry is 0-0.6 V, and the scan rate is 5-50 mV s -1 , the number of scanning circles is 10 to 100 circles.
[0025] The third aspect of the present invention proposes the use of the above-mentioned nanoporous nickel-nickel oxide loaded silver nanoflower material as a supercapacitor electrode material.
[0026] The present invention has the following beneficial effects:
[0027] (1) The method of the present invention utilizes the principle that Ni and Ag elements are immiscible at room temperature, creatively adds Ag element to the nickel-based amorphous alloy, and successfully prepares a silver-containing nickel-based amorphous alloy, whose composition is relatively uniform. After dealloying, a supersaturated nanoporous nickel-silver alloy is obtained, which provides favorable conditions for the subsequent electrochemical activation and precipitation of silver nanoflowers. The preparation method of the alloy breaks through the limitations of the molding ability of traditional crystalline alloys.
[0028] (2) Compared with the disclosed single nanoporous nickel-nickel oxide electrode material preparation patent, the method of the present invention prepares a nanoporous nickel-nickel oxide loaded silver nanoflower composite electrode sheet. The silver nanoflower not only increases the conductivity of the electrode material, but also improves the interface wettability between the electrode material and the electrolyte, increases the surface area of the electrode material, and thus greatly improves its rate capability and specific capacitance.
[0029] (3) The prepared highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material is an integrated material, avoiding the use of conductive agents and adhesives. The silver nanoflowers are composed of silver nanosheets or silver nanoparticles, which are evenly distributed on the surface of the nanoporous nickel-nickel oxide. The diameter of the silver nanoflowers is 0.5 to 3 μm, the size of the silver nanosheets is 0.2 to 1.5 μm, and the diameter of the silver nanoparticles is 0.1 to 0.5 μm;
[0030] (4) Silver nanoflowers not only increase the conductivity of the electrode material, but also improve the interfacial wettability of the electrode / electrolyte, greatly improving the rate performance and specific capacitance of the electrode material. When the current density increases by 64 times, its capacitance retention rate is still as high as more than 95%, and the maximum specific capacitance reaches 1264.3F cm -3 ;
[0031] (5) The present invention skillfully combines the dealloying technology and the electrochemical activation technology to prepare a highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material. In the preparation process, the dealloying does not require the use of a highly toxic hydrofluoric acid solution, and the safety is relatively high. The electrochemical activation technology plays a role in precipitating the silver element and further oxidizing the nanoporous nickel. The preparation process has a short cycle, and the prepared composite material has good mechanical integrity, can be recycled and reused, and the economic benefits are improved.
[0032] (6) The preparation method of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflowers of the present invention has the advantages of being simple and gentle, having high repeatability and reproducibility of materials, and having low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a scanning electron microscope photograph of the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared in Example 1.
[0034] Figure 2 This is the energy spectrum analysis diagram of the silver nanoflowers loaded with nanoporous nickel-nickel oxide prepared in Example 1.
[0035] Figure 3 This is the XRD spectrum of the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared in Example 1.
[0036] Figure 4 This is the constant current charge and discharge curve of the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared in Example 1.
[0037] Figure 5 This is a scanning electron microscope photograph of the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared in Example 2.
[0038] Figure 6 This is a scanning electron microscope photograph of the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared in Example 3. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0041] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0042] Embodiment 1:
[0043] A nanoporous nickel-nickel oxide loaded silver nanoflower material, the material is composed of a silver-containing nickel-based amorphous alloy, a nanoporous nickel-nickel oxide layer and silver nanoflowers; the silver-containing nickel-based amorphous alloy is used as the middle core layer, nanoporous nickel-nickel oxide layers are arranged on both sides of the middle core layer, and the outermost layer is silver nanoflowers; the silver nanoflowers are composed of silver nanosheets or silver nanoparticles, uniformly distributed on the surface of the nanoporous nickel-nickel oxide, the diameter of the silver nanoflowers is 0.5 to 3 μm, the size of the silver nanosheets is 0.2 to 1.5 μm, and the diameter of the silver nanoparticles is 0.1 to 0.5 μm. The composition of the silver-containing nickel-based amorphous alloy is Ni 30 Zr 60 Ag 10 The thickness ratio of the silver-containing nickel-based amorphous alloy core layer, the nanoporous nickel-nickel oxide layer, and the silver nanoflower is 2:2:1.
[0044] The preparation method comprises the following steps:
[0045] The first step is to prepare a silver-containing nickel-based amorphous alloy strip
[0046] According to the target alloy Ni 30 Zr 60 Ag 10 The atomic percentage of each element in the master alloy is 99.9wt.% of pure Ni 4.236g, pure Zr 13.169g, and pure Ag 2.595g, respectively, and 20g of the master alloy raw material is obtained by mixing. Then the mixed metal raw materials are placed in a vacuum arc furnace, and 20g of pure Ti with a purity of 99.9wt.% is placed in the vacuum arc furnace independently without contacting with the master alloy raw materials, and is melted as a deoxidizing material; under the protection of argon, the master alloy is repeatedly melted 4 times, each time for about 30 seconds, to ensure the uniformity of the alloy structure; after the melting is completed, it is cooled to room temperature with the furnace to obtain Ni 30 Zr 60 Ag 10 Alloy ingot.
[0047] The alloy ingot obtained after smelting was descaled and cut into suitable sizes, placed in a quartz tube and cleaned with anhydrous ethanol. Amorphous alloy ribbons were prepared using a vacuum spinning machine. The preparation parameters were: vacuum degree 9.0×10 - 4 Pa, blowing pressure 0.1MPa, copper roller surface speed 36m s -1 The master alloy was placed in a quartz tube, heated to a molten state under an argon protective atmosphere, and blow-cast to form an amorphous alloy strip, thereby preparing a silver-containing nickel-based amorphous alloy strip with a thickness of 20 μm and a width of 2 mm;
[0048] The second step is to prepare nanoporous nickel-silver alloy by dealloying
[0049] A mixed solution of 0.05M NH4F and 0.05M H3PO4 was prepared, 5cm of the above silver-containing nickel-based amorphous alloy strip was cut, and 2cm of it was immersed in the mixed solution for dealloying treatment for 4h at room temperature. The remaining 3cm of the strip was used as an electrode lead, and then the sample was taken out and repeatedly rinsed with deionized water for 3 times to obtain a supersaturated nanoporous nickel-silver alloy;
[0050] Step 3: Preparation of nanoporous nickel-nickel oxide-loaded silver nanoflowers by electrochemical activation
[0051] The supersaturated nanoporous nickel-silver alloy prepared in the second step was placed in a 1 M KOH solution and electrochemically activated by cyclic voltammetry (CV) in a three-electrode system. The potential window of CV was 0-0.6 V and the scan rate was 10 mV s -1 , the scanning number is 50 circles, and silver nanoflowers supported by nanoporous nickel-nickel oxide are obtained;
[0052] In order to detect the electrochemical properties of the prepared electrode materials, an electrochemical workstation was used to test its constant current charge and discharge performance in a three-electrode system. The test electrolyte was 2 mol L -1 The KOH solution prepared above was used as the working electrode, the platinum mesh electrode was used as the auxiliary electrode, and the Ag / AgCl electrode was used as the reference electrode. The current density of the constant current charge and discharge was 1A cm -3 , the voltage window is 0~0.45V.
[0053] Figure 1 This is a scanning electron microscope photo of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material in this embodiment. The silver nanoflower prepared in this example is composed of many silver nanoparticles and silver nanosheets. The diameter of the silver nanoflower is 0.5-2μm, the size of the silver nanosheet is 0.2-1μm, and the diameter of the silver nanoparticle is 0.1-0.4μm; the silver nanoflower is evenly distributed on the surface of the nanoporous nickel-nickel oxide, and the coverage rate of the silver nanoflower in the region on the electrode surface reaches more than 50% (area share). The silver nanoflower improves the conductivity of the electrode material and greatly improves its electrochemistry.
[0054] Figure 2 This is the energy spectrum analysis diagram of the nanoflower-like structure in the electrode material in this embodiment. A strong peak of metallic silver appears in the diagram, indicating that the main component of the flower-like structure prepared in this example is silver, proving that silver element is precipitated after electrochemical activation of the supersaturated nickel-silver alloy.
[0055] Figure 3This is the XRD spectrum of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material obtained in this example. The peaks of metal Ni and NiO are clearly seen in the figure, indicating that the Zr and Ti elements on the surface of the strip are basically selectively dissolved during the dealloying process, and NiO is generated during the electrochemical activation. At the same time, the presence of some amorphous bun peaks indicates that the electrode retains a certain amorphous core layer, giving the electrode structural integrity. Figure 2 From the energy spectrum of the nanoflower-like structure, it can be seen that through the two processes of dealloying and electrochemical activation, a highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material was successfully prepared.
[0056] Figure 4 The constant current charge and discharge curve of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material in this embodiment is shown in Figure 1. The charging and discharging platforms can be clearly seen from the curve, which correspond to the oxidation reaction and the reduction reaction, respectively, indicating its pseudocapacitive characteristics. -3 The specific capacitance is as high as 1264.3F cm at the current density -3 .
[0057] Embodiment 2:
[0058] A nanoporous nickel-nickel oxide loaded silver nanoflower material, the material is composed of a silver-containing nickel-based amorphous alloy, a nanoporous nickel-nickel oxide layer and silver nanoflowers; the silver-containing nickel-based amorphous alloy is used as the middle core layer, nanoporous nickel-nickel oxide layers are arranged on both sides of the middle core layer, and the outermost layer is silver nanoflowers; the silver nanoflowers are composed of silver nanosheets or silver nanoparticles, uniformly distributed on the surface of the nanoporous nickel-nickel oxide, the diameter of the silver nanoflowers is 0.5 to 3 μm, the size of the silver nanosheets is 0.2 to 1.5 μm, and the diameter of the silver nanoparticles is 0.1 to 0.5 μm. The composition of the silver-containing nickel-based amorphous alloy is Ni 30 Ti 60 Ag 10 The thickness ratio of the silver-containing nickel-based amorphous alloy core layer, the nanoporous nickel-nickel oxide layer, and the silver nanoflower is 2:1:1.
[0059] The preparation method comprises the following steps:
[0060] The first step is to prepare a silver-containing nickel-based amorphous alloy strip
[0061] According to the target alloy Ni 30 Ti 60 Ag 10The atomic percentage of each element in the master alloy is 99.9wt.% of pure Ni 6.165g, pure Ti 10.058g and pure Ag 3.777g, respectively, and 20g of the master alloy raw material is mixed. Then the mixed metal raw materials are placed in a vacuum arc furnace, and 20g of pure Ti with a purity of 99.9wt.% is placed in the vacuum arc furnace independently without contacting with the master alloy raw material, and is melted as a deoxidizing material; under the protection of argon, the master alloy is repeatedly melted 4 times, each time for about 30 seconds, to ensure the uniformity of the alloy structure; after the melting is completed, it is cooled to room temperature with the furnace to obtain Ni 30 Ti 60 Ag 10 Alloy ingot.
[0062] The alloy ingot obtained after smelting was descaled and cut into suitable sizes, placed in a quartz tube and cleaned with anhydrous ethanol. Amorphous alloy thin strips were prepared using a vacuum stripping machine. The preparation conditions were: vacuum degree 9.0×10 - 4 Pa, blowing pressure 0.1MPa, copper roller speed 36m s -1 The master alloy was placed in a quartz tube, heated to a molten state under an argon protective atmosphere, and blow-cast to form an amorphous alloy strip, preparing an alloy strip with a thickness of 20 μm and a width of 2 cm;
[0063] The second step is to prepare nanoporous nickel-silver alloy by dealloying
[0064] A mixed solution of 0.1M NH4F and 0.1M H3PO4 was prepared, 5cm of the above silver-containing nickel-based amorphous alloy strip was cut, and 2cm of it was immersed in the mixed solution for dealloying for 3h at room temperature. The remaining 3cm of the strip was used as an electrode lead, and then the sample was taken out and repeatedly rinsed with deionized water for 3 times to obtain a supersaturated nanoporous nickel-silver alloy;
[0065] Step 3: Preparation of nanoporous nickel-nickel oxide-loaded silver nanoflowers by electrochemical activation
[0066] The supersaturated nanoporous nickel-silver alloy prepared in the second step was placed in a 1 M NaOH solution and electrochemically activated by cyclic voltammetry (CV) in a three-electrode system. The potential window of CV was 0-0.6 V and the scan rate was 20 mV s -1 , the scanning number is 80 circles, and silver nanoflowers supported by nanoporous nickel-nickel oxide are obtained;
[0067] In order to detect the electrochemical properties of the prepared electrode materials, an electrochemical workstation was used to test its constant current charge and discharge performance in a three-electrode system. The test electrolyte was 2 mol L -1The KOH solution prepared above was used as the working electrode, the platinum mesh electrode was used as the auxiliary electrode, and the Ag / AgCl electrode was used as the reference electrode. The current density of the constant current charge and discharge was 1A cm -3 , the voltage window is 0~0.45V.
[0068] The diameter of the silver nanoflowers prepared in this embodiment is 0.6-2.5 μm, the size of the silver nanosheets is 0.8-1.1 μm, and the diameter of the silver nanoparticles is 0.3-0.5 μm; the silver nanoflowers are evenly distributed on the surface of the nanoporous nickel-nickel oxide, and the coverage rate of the silver nanoflowers in the region on the electrode surface reaches more than 60% (area share).
[0069] The electrochemical performance of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material in this embodiment was tested. The results showed that: 3 At a current density of 1.547 W, the specific capacitance reaches 1156.4.3 F cm -3 .
[0070] Embodiment 3:
[0071] A nanoporous nickel-nickel oxide loaded silver nanoflower material, the material is composed of a silver-containing nickel-based amorphous alloy, a nanoporous nickel-nickel oxide layer and silver nanoflowers; the silver-containing nickel-based amorphous alloy is used as the middle core layer, nanoporous nickel-nickel oxide layers are arranged on both sides of the middle core layer, and the outermost layer is silver nanoflowers; the silver nanoflowers are composed of silver nanosheets or silver nanoparticles, uniformly distributed on the surface of the nanoporous nickel-nickel oxide, the diameter of the silver nanoflowers is 0.5 to 3 μm, the size of the silver nanosheets is 0.2 to 1.5 μm, and the diameter of the silver nanoparticles is 0.1 to 0.5 μm. The composition of the silver-containing nickel-based amorphous alloy is Ni 30 Zr 20 Ti 40 Ag 10 The thickness ratio of the silver-containing nickel-based amorphous alloy core layer, the nanoporous nickel-nickel oxide layer, and the silver nanoflower is 2:3:1.
[0072] The first step is to prepare a silver-containing nickel-based amorphous alloy strip
[0073] According to the target alloy Ni 30 Zr 20 Ti 40 Ag 10The atomic percentage of each element in the master alloy is 99.9wt.% of pure Ni 5.353g, pure Zr 5.546g, pure Ti 5.822g, and pure Ag 3.279g, respectively, and 20g of the master alloy raw material is mixed. Then the mixed metal raw materials are placed in a vacuum arc furnace, and 20g of pure Ti with a purity of 99.9wt.% is placed in the vacuum arc furnace independently without contacting the master alloy raw materials, and is melted as a deoxidizing material; under the protection of argon, the master alloy is repeatedly melted 4 times, each time for about 30 seconds, to ensure the uniformity of the alloy structure; after the melting is completed, it is cooled to room temperature with the furnace to obtain Ni 30 Zr 20 Ti 40 Ag 10 Alloy ingot.
[0074] The alloy ingot obtained after smelting was descaled and cut into suitable sizes, placed in a quartz tube and cleaned with anhydrous ethanol. Amorphous alloy ribbons were prepared using a vacuum spinning machine. The preparation conditions were: vacuum degree 9.0×10 - 4 Pa, blowing pressure 0.1MPa, copper roller speed 36m s -1 The master alloy was placed in a quartz tube, heated to a molten state under an argon protective atmosphere, and blow-cast to form an amorphous alloy strip, preparing an alloy strip with a thickness of 20 μm and a width of 2 cm;
[0075] The second step is to prepare nanoporous nickel-silver alloy by dealloying
[0076] A mixed solution of 0.2M NH4F and 0.2M H3PO4 was prepared, 5cm of the above silver-containing nickel-based amorphous alloy strip was cut, and it was immersed in the mixed solution for 2cm for dealloying treatment for 1h at room temperature. The remaining 3cm strip was used as an electrode lead, and then the sample was taken out and repeatedly rinsed with deionized water for 3 times to obtain a supersaturated nanoporous nickel-silver alloy;
[0077] Step 3: Preparation of nanoporous nickel-nickel oxide-loaded silver nanoflowers by electrochemical activation
[0078] The supersaturated nanoporous nickel-silver alloy prepared in the second step was placed in a 2M KOH solution and electrochemically activated by cyclic voltammetry (CV) in a three-electrode system. The potential window of CV was 0-0.6 V and the scan rate was 30 mV s -1 , the scanning circle number is 60 circles, and the silver nanoflowers supported by nanoporous nickel-nickel oxide are obtained;
[0079] In order to detect the electrochemical properties of the prepared electrode materials, an electrochemical workstation was used to test its constant current charge and discharge performance in a three-electrode system. The test electrolyte was 2 mol L -1The KOH solution prepared above was used as the working electrode, the platinum mesh electrode was used as the auxiliary electrode, and the Ag / AgCl electrode was used as the reference electrode. The current density of the constant current charge and discharge was 1A cm -3 , the voltage window is 0~0.45V.
[0080] The diameter of the silver nanoflowers prepared in this embodiment is 0.7-2.6 μm, the size of the silver nanosheets is 0.6-1.3 μm, and the diameter of the silver nanoparticles is 0.2-0.3 μm; the silver nanoflowers are evenly distributed on the surface of the nanoporous nickel-nickel oxide, and the coverage rate of the silver nanoflowers in the region on the electrode surface reaches more than 60% (area share).
[0081] The electrochemical performance of the highly conductive nanoporous nickel-nickel oxide loaded silver nanoflower electrode material in this embodiment was tested. The results showed that: 3 At a current density of 1.34 W, the specific capacitance reaches 1095.4 F cm -3 .
[0082] Comparative Example 1:
[0083] The prepared supersaturated nanoporous nickel-silver alloy was placed in a 1M KOH solution, and the number of cyclic voltammetry cycles was set to less than 10 cycles. Other conditions were the same as those in Example 1. The scanning electron microscopy results showed that silver was precipitated on the electrode surface only in the form of particles with a size of about a dozen nanometers, and did not aggregate into silver nanoflowers. Figure 5 Electrochemical tests showed that the electrode has a -3 At a current density of 1.38 W, the specific capacitance is only 863.2 Fcm -3 .
[0084] Comparative Example 2:
[0085] The prepared supersaturated nanoporous nickel-nickel oxide was placed in a 1M KOH solution, and the number of cyclic voltammetry cycles was set to more than 100 cycles. Other conditions were the same as in Example 1. The results showed that no silver nanoflowers were found on the surface of the nanoporous nickel-nickel oxide, indicating that the electrochemical activation time was long, the size of the silver nanoflowers was too large, and they had fallen off the electrode surface. The electrochemical test found that the electrode was -3 At a current density of 1.38 W, the specific capacitance is only 605.6 Fcm -3 .
[0086] Comparative Example 3:
[0087] The prepared silver-containing nickel-based amorphous alloy strip was dealloyed in a mixture of 0.6M NH4F and 0.6M H3PO4, with other conditions being the same as in Example 2. The scanning electron microscopy results showed that large cracks appeared on the surface of the electrode, and its mechanical properties were very poor, it was easy to break, and it was difficult to be self-supporting. Figure 6 shown.
[0088] Comparative Example 4:
[0089] The target alloy is a Ni-Zr-Ti-Ag amorphous alloy with a silver content of more than 10 at.%, and other conditions are the same as those in Example 3. It is found that the amorphous alloy strips just thrown out are brittle and easy to break; after dealloying, the sample corrodes and breaks into small pieces, and the mechanical integrity of the initial strips cannot be maintained.
[0090] The above comparative examples are all cases of experimental failure, which shows that any change in the preparation process will lead to experimental results that cannot meet expectations. When preparing silver-containing nickel-based amorphous alloys, the atomic percentage of silver elements should be controlled between 5% and 10%, otherwise the prepared strips will be brittle; when dealloying, attention should be paid to controlling the concentration ratio of the etching solution and the dealloying time; during electrochemical activation, the parameters of cyclic voltammetry should be strictly controlled within a reasonable range, otherwise it will be difficult to obtain uniformly distributed and appropriately sized silver nanoflowers. Only by strictly controlling the parameters of each process link can we successfully obtain nanoporous nickel-nickel oxide loaded silver nanoflower electrode materials with excellent electrochemical properties and high conductivity.
[0091] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A nanoporous nickel-nickel oxide loaded silver nanoflower material, characterized in that: The material is composed of a silver-containing nickel-based amorphous alloy, a nanoporous nickel-nickel oxide layer and silver nanoflowers; the silver-containing nickel-based amorphous alloy is used as an intermediate core layer, nanoporous nickel-nickel oxide layers are arranged on both sides of the intermediate core layer, and the outermost layer is a silver nanoflower; the silver nanoflower is composed of silver nanosheets or silver nanoparticles, and is evenly distributed on the surface of the nanoporous nickel-nickel oxide; the silver-containing nickel-based amorphous alloy is composed of Ni 40-x (Zr,Ti) 60 Ag x , where the subscripts are the atomic percentages of the elements, 5≤x≤10.
2. The nanoporous nickel-nickel oxide loaded silver nanoflower material according to claim 1, characterized in that: The diameter of the silver nanoflower is 0.5-3 μm, the size of the silver nanosheet is 0.2-1.5 μm, and the diameter of the silver nanoparticle is 0.1-0.5 μm.
3. The nanoporous nickel-nickel oxide loaded silver nanoflower material according to claim 1, characterized in that: The thickness ratio of the silver-containing nickel-based amorphous alloy core layer, the nanoporous nickel-nickel oxide layer, and the silver nanoflower is 2:1 to 3:
1.
4. The nanoporous nickel-nickel oxide loaded silver nanoflower material according to claim 1, characterized in that: The composition of the silver-containing nickel-based amorphous alloy is Ni 30 Zr 60 Ag 10 、Ni 30 Ti 60 Ag 10 or Ni 30 Zr 20 Ti 40 Ag 10 .
5. The method for preparing the nanoporous nickel-nickel oxide loaded silver nanoflower material according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Preparation of Ni-Zr / Ti-Ag or Ni-Zr-Ti-Ag amorphous alloy strips: According to the composition of the silver-containing nickel-based amorphous alloy, Ni, Zr / Ti, Ag or Ni, Zr, Ti, Ag are mixed, and the mixed alloy raw materials are evenly melted to obtain a Ni-Zr / Ti-Ag or Ni-Zr-Ti-Ag alloy ingot; the obtained alloy ingot is heated to a molten state, and the alloy liquid is blown out by an inert gas, so that the molten liquid metal solidifies on a rotating copper roller to obtain a silver-containing nickel-based amorphous alloy strip; (2) Dealloying to prepare supersaturated nanoporous nickel-silver alloy: placing a silver-containing nickel-based amorphous alloy strip in an acid solution, then taking it out and washing it to obtain a supersaturated nanoporous nickel-silver alloy; (3) Preparation of nanoporous nickel-nickel oxide-loaded silver nanoflowers by electrochemical activation: The supersaturated nanoporous nickel-silver alloy is placed in an alkaline solution and electrochemically activated by cyclic voltammetry (CV) to obtain a nanoporous nickel-nickel oxide-loaded silver nanoflower material.
6. The preparation method according to claim 1, characterized in that: The purity of Ni, Ti, Zr and Ag is 99.9wt.%; the rotation speed of the copper roller is 34-36m / s.
7. The preparation method according to claim 1, characterized in that: The silver-containing nickel-based amorphous alloy strip has a thickness of 20 to 50 μm and a width of 1.5 to 2 cm.
8. The preparation method according to claim 1, characterized in that: The acid solution is a mixture of H3PO4 and NH3F, wherein the concentrations of NH3F and H3PO4 are both 0.02-0.5M, and the molar ratio of H3PO4 to NH3F is 1:1; the alkali solution is a NaOH or KOH solution, and the concentration is 1-6M.
9. The preparation method according to claim 1, characterized in that: The potential window of the cyclic voltammetry is 0-0.6 V, and the scan rate is 5-50 mV s -1 , the number of scanning circles is 10 to 100 circles.
10. Use of the nanoporous nickel-nickel oxide loaded silver nanoflower material as described in any one of claims 1 to 4 or the nanoporous nickel-nickel oxide loaded silver nanoflower material prepared by the preparation method as described in any one of claims 5 to 9 as a supercapacitor electrode material.
Citation Information
Patent Citations
Nano-porous copper silver supported manganese dioxide electrode slice and preparation method therefor
CN104867681A
Nanometer porous nickel / nickel oxide supercapacitor electrode material and preparation method thereof
CN107240507A
Fabrication method of penetrating base perpendicular transistor
CN107452877A
Composite electrode material based on Ti-Cu-Ag amorphous alloy and preparation method thereof