Spherical graphite material and preparation method thereof, negative plate and battery

Through the core-shell structure of spherical graphite material and the composite adhesive process, the low energy density and safety hazards of lithium-ion batteries during fast charging are solved, and the high capacity and fast charging are achieved, and the mechanical strength of the material is improved. Electrochemical properties.

CN119050347APending Publication Date: 2024-11-29CARBON ONE NEW ENERGY HANGZHOU CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411106533.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The graphite anode materials of existing lithium-ion batteries have problems of low energy density and safety hazards during fast charging, and the secondary granulation process is difficult to control, resulting in high costs and high process barriers.

Method used

Spherical graphite material is used, which is a core-shell structure, the shell is an amorphous carbon layer, and the core is graphite secondary particles. It is prepared by spray drying and vacuum impregnation processes, combined with the combination of low-temperature and high-temperature binders to form high density and High isotropic particles.

Benefits of technology

It realizes fast charging while improving specific capacity, taking into account fast charging and high capacity, reducing irreversible capacity, improving the mechanical strength and electrochemical performance of the material, and solving the problems of low energy density and safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050347A_ABST
    Figure CN119050347A_ABST
Patent Text Reader

Abstract

The invention provides a spherical graphite material and a preparation method thereof, a negative electrode plate and a battery, and relates to the technical field of negative electrode materials. The spherical graphite material is of a core-shell structure, a shell is an amorphous carbon layer, an inner core is graphite secondary particles, the graphite secondary particles are formed by granulation of graphite primary particles, soft carbon and hard carbon are distributed among the graphite primary particles, the hard carbon is formed by carbonization of a low-temperature binder, and the soft carbon is formed by carbonization of a high-temperature binder. The spherical graphite material has excellent fast charging performance, high energy density and excellent cycling stability, and can give consideration to both fast charging and large capacity when being used as a negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium battery negative electrode materials, and in particular to a spherical graphite material and a preparation method thereof, a negative electrode sheet and a battery. Background Art

[0002] With the rapid popularization of electric vehicles in the global market and people's more stringent requirements for consumer electronics, fast charging technology is an inevitable trend of historical development. However, current high-energy lithium-ion batteries (LIBs) cannot support ultra-fast power input without any adverse consequences. The capacity decay and safety hazards of graphite anodes are key technical barriers to fast charging technology. The development of graphite anode materials that can achieve fast charging is crucial for the sustainable large-scale commercial application of lithium-ion batteries.

[0003] The layered structure of graphite material determines that lithium ions must be embedded from the end face of the material and gradually diffuse into the interior of the particles, resulting in a longer diffusion path, while the smaller interlayer spacing makes the diffusion rate of lithium ions lower and the rate performance is poor. In addition, during fast charging, lithium ions are easily deposited on the graphite surface to form lithium dendrites, leading to serious safety hazards. Generally speaking, the orientation of graphite materials in electrodes should be as perpendicular to the current collector as possible, that is, it is hoped that the material has a high degree of isotropy, which is conducive to reducing the resistance to lithium ion embedding and improving the rate charging performance. In terms of particle size, it is generally believed that small-particle graphite has better rate charging performance. However, the smaller the particle size, the larger the specific surface area, and the larger the irreversible capacity of the material. Secondary granulation is an important process that high-end artificial graphite often takes in order to balance rate performance and energy density. The secondary particles prepared by granulation have a high degree of isotropy, and at the same time have the advantages of high compaction density and large capacity of large particles, and the advantages of large specific surface area and multiple lithium ion deintercalation channels of small particles, so as to balance rate performance and energy density.

[0004] However, the particle distribution and fine powder of secondary granulation are difficult to control, resulting in high cost and high process barriers. Summary of the invention

[0005] The present invention provides a spherical graphite material and a secondary granulation method thereof. The graphite material prepared by the method can be used as a negative electrode material for a battery, can achieve fast charging while improving specific capacity, and takes both fast charging and high capacity into consideration, thus solving the problem of low energy density of graphite materials during fast charging in the prior art.

[0006] On the one hand, the present invention provides a spherical graphite material that can be used as a negative electrode material and can take into account both fast charging and capacity.

[0007] The present invention provides a spherical graphite material, which is a core-shell structure, wherein the shell is an amorphous carbon layer, the core is secondary graphite particles, the secondary graphite particles are granulated from primary graphite particles, soft carbon and hard carbon are distributed between the primary graphite particles, the hard carbon is formed by carbonization of a low-temperature binder, and the soft carbon is formed by carbonization of a high-temperature binder.

[0008] Furthermore, the median particle size D of the spherical graphite material is 50 10-30μm.

[0009] Furthermore, the compaction density of the spherical graphite material is 1-2 g / cm 3 . Preferably 1.4-1.8g / cm 3 .

[0010] Furthermore, the OI value of the spherical graphite material is 0.4-1.

[0011] Furthermore, the sphericity of the spherical graphite material is ≥0.75; preferably ≥0.80.

[0012] Furthermore, the median particle size D of the graphite primary particles is 50 2-8μm.

[0013] Furthermore, the low-temperature binder is one or more of carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone or polyacrylic acid.

[0014] Furthermore, the high temperature adhesive is asphalt.

[0015] Furthermore, the median particle size D of the high temperature binder is 50 0.5-5μm.

[0016] Furthermore, the mass ratio of the graphite primary particles, the high-temperature binder and the low-temperature binder is 1-10:0.1-2:0.1-2.

[0017] Furthermore, soft carbon and a small amount of hard carbon are distributed between the graphite primary particles, that is, the content of hard carbon between the graphite primary particles is lower than that of soft carbon.

[0018] Furthermore, the amorphous carbon layer is formed by carbonization of a coating agent. A suitable coating agent is emulsified asphalt or fluidized asphalt. In the spherical graphite material, the surface of the graphite secondary particles is coated with a coating agent, and the coating agent is filled between adjacent graphite primary particles and adjacent graphite secondary particles, and the amorphous carbon layer is formed by carbonization of the coating agent coated on the surface of the graphite secondary particles.

[0019] Furthermore, the mass ratio of the graphite secondary particles to the coating agent is 100:(1-100).

[0020] In another aspect, the present invention provides a method for preparing a spherical graphite material, the method comprising the following steps:

[0021] S1, dispersing graphite primary particles, a high temperature binder, a low temperature binder, and a stabilizer in water to prepare a slurry, and then spray drying to obtain a graphite secondary particle precursor;

[0022] S2, heat-treating the graphite secondary particle precursor under a protective gas atmosphere to obtain graphite secondary particles;

[0023] S3, vacuum impregnating the graphite secondary particles with the coating agent;

[0024] S4, carbonizing the product after vacuum impregnation.

[0025] Furthermore, in step S1, the low-temperature binder is one or more of carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone or polyacrylic acid;

[0026] Furthermore, the high temperature adhesive is asphalt.

[0027] Furthermore, the stabilizer is one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran, polyethylene oxide or polypropylene oxide.

[0028] Furthermore, the median particle size D of the graphite primary particles is 50 2-8μm.

[0029] Furthermore, the median particle size D of the high temperature binder is 50 0.5-5μm.

[0030] Furthermore, the mass ratio of the graphite primary particles, the high-temperature binder, the low-temperature binder, the stabilizer and water is 1-10: 0.1-2: 0.1-2: 0.1-2: 1-100.

[0031] Furthermore, in step S1: firstly add a low-temperature binder and a stabilizer into water, stir and dissolve, then add graphite primary particles and a high-temperature binder, continue stirring to form a slurry; and then spray dry to obtain a graphite secondary particle precursor.

[0032] Furthermore, in step S1: the inlet temperature of the spray drying is 200-300°C, and the outlet temperature is 100-130°C.

[0033] Further, in step S2: the heat treatment is a gradient temperature rise heat treatment, the heat treatment temperature in the first stage is 100-300° C., and the heat treatment time in the first stage is 0.5-4h;

[0034] The second stage heat treatment temperature is 500-1000℃, and the second stage heat treatment time is 1-8h;

[0035] Further, in step S2, the heating rate of the heat treatment is 2-10°C / min;

[0036] Furthermore, in step S2, the heat treatment is performed under a protective gas atmosphere, and the protective gas is one or more of nitrogen, argon, xenon, helium, and neon.

[0037] Further, in step S3: the vacuum impregnation is performed under a protective gas atmosphere, and the protective gas is one or more of nitrogen, argon, xenon, helium, and neon;

[0038] Furthermore, the coating agent is emulsified asphalt or fluidized asphalt, and the fluidized asphalt is prepared by dissolving asphalt in gasoline, diesel, benzene, chloroform or carbon tetrachloride.

[0039] Furthermore, the mass ratio of the spherical secondary particles to the coating agent is 100:(1-100).

[0040] Furthermore, the vacuum impregnation time is 0.5-50h.

[0041] Further, in step S4, the carbonization is carried out under a protective gas atmosphere, and the protective gas is one or more of nitrogen, argon, xenon, helium, and neon;

[0042] And / or, the carbonization temperature is 1100-1300° C., and the carbonization time is 4-24 hours.

[0043] The present invention also provides an application of any of the above spherical graphite materials in a battery as a negative electrode material. The present invention provides a negative electrode sheet, comprising any of the above spherical graphite materials or a spherical graphite material prepared by any of the above methods.

[0044] In another aspect, the present invention provides a lithium-ion battery, comprising any of the above-mentioned negative electrode sheets or a negative electrode thereof made of any of the above-mentioned spherical graphite materials.

[0045] Compared with the prior art, the present invention has the following advantages:

[0046] 1. The present invention provides a secondary granulation process for spherical graphite materials. In the secondary granulation, the type and amount of the binder are crucial to the formation of particles and the performance of the final material. The binder should not only promote the bonding between particles, but also form amorphous carbon in the subsequent sintering process to fill the gaps between particles, improve the densification of graphite, and reduce the irreversible capacity. However, excessive binder will lead to increased porosity and affect the electrochemical properties of the material. The prior art generally uses asphalt as a binder, while the present invention uses a "composite" binder. Asphalt is used as a high-temperature binder to play a binder role in the process after spray drying; low-temperature binder is used to play a binder role in the process of slurry adjustment and spray drying. On the one hand, it plays a role in stabilizing the slurry during the slurry adjustment process, making the slurry more uniform while maintaining a long time without sedimentation and stratification, increasing the probability of ball formation; more importantly, a curing reaction occurs during the spray drying process to play a bonding role.

[0047] 2. During the secondary granulation process, the average size and particle size distribution of the particles need to be precisely controlled to ensure the performance consistency of the final product. Too large or unevenly distributed particle sizes will lead to uneven pore size and distribution in the finished product, affecting the mechanical strength and conductivity of the material. The ideal secondary granulation should generate particles with moderate particle size and narrow distribution to improve the compaction density and cycle stability of the material. The spherical graphite material obtained by the secondary granulation of the present invention has a mean particle size D 50 10-30μm, compacted density 1-2g / cm 3 , OI value is 0.4-1, and sphericity is ≥0.75, which can take into account both fast charging and capacity.

[0048] 3. The particle shape after secondary granulation has a direct impact on the compaction density and pore structure of the material. Irregular particle shape and wide particle size distribution will reduce the compaction density and increase the difficulty of subsequent electrode processing, and the unevenly distributed pore structure will reduce the electrochemical performance of the material. Through the secondary granulation process of the present invention, graphite secondary particles with regular shape, high sphericity and stable structure can be obtained, and a high overall open porosity and mechanical strength are maintained, which is conducive to the subsequent processing of the electrode.

[0049] 4. The secondary granulation process of the present invention, under the synergistic effect of formula adjustment and process optimization, uses spray drying to obtain a spherical particle precursor with a very high degree of isotropy, laying a good foundation for the preparation of artificial graphite negative electrode materials with ultra-high rate and long cycle. The vacuum impregnation process immerses the fluidized asphalt into the particle pores of the spherical particle precursor to densify it, produce greater bonding strength and reduce the specific surface area. It avoids the reduction of the first effect and capacity due to the generation of a large amount of solid electrolyte interface film (SEI film) due to excessively high specific surface area. The spherical artificial graphite prepared by a series of processes such as spray drying ball making, high temperature curing, vacuum impregnation, etc. has excellent rate performance and cycle stability.

[0050] 5. The spherical graphite material of the present invention is a core-shell structure, the shell is an amorphous carbon layer, the core is a graphite secondary particle, the graphite secondary particle is granulated from graphite primary particles, soft carbon and a small amount of hard carbon are distributed between the graphite primary particles, the hard carbon is formed by carbonization of a low-temperature binder, and the soft carbon is formed by carbonization of a high-temperature binder. The structure and good cycle stability of graphite are improved by soft carbon, and the high specific capacity, porous structure and good battery performance of graphite are improved by hard carbon. The mixed design of soft carbon and hard carbon can improve the rate performance and cycle performance of graphite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0052] Figure 1 This is a SEM image of the spherical graphite material described in the embodiment of the present invention.

[0053] Figure 2 A schematic flow chart of a method for preparing a spherical graphite material provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0054] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] During fast charging, lithium ions tend to deposit on the graphite surface to form lithium dendrites, leading to serious safety hazards. Generally speaking, the orientation of graphite materials in electrodes should be as perpendicular to the current collector as possible, that is, it is hoped that the material has a high degree of isotropy, which is conducive to reducing the resistance to lithium ion embedding and improving rate charging performance. In terms of particle size, it is generally believed that small-particle graphite has better rate charging performance. However, the smaller the particle size, the larger the specific surface area, and the larger the irreversible capacity of the material. How to balance fast charging and capacity has always been a difficult problem in the application of graphite materials in the battery field.

[0056] One embodiment of the present invention provides a spherical graphite material. The spherical graphite material is a core-shell structure (such as Figure 1 As shown in the figure, a spherical core-shell structure), the shell is an amorphous carbon layer, the core is a graphite secondary particle, wherein the graphite secondary particle is granulated from graphite primary particles (graphite raw materials), soft carbon and hard carbon are distributed between the graphite primary particles, the donor of the hard carbon is a low-temperature binder, and the donor of the soft carbon is a high-temperature binder.

[0057] In the embodiment of the present invention, the soft carbon may be formed by carbonizing a high temperature binder. The high temperature binder may be a soft carbon donor. An applicable high temperature binder may be asphalt.

[0058] In the embodiment of the present invention, the hard carbon is formed by carbonizing a low temperature binder. The low temperature binder is a hard carbon donor. The applicable low temperature binder may be one or more of carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone or polyacrylic acid.

[0059] In the embodiment of the present invention, soft carbon and a small amount of hard carbon are distributed between the graphite primary particles. The content of hard carbon between the graphite primary particles is lower than that of soft carbon. The mixed design of soft carbon and hard carbon can improve the rate performance and cycle performance of graphite materials.

[0060] In the embodiment of the present invention, the mass ratio of graphite primary particles, high temperature binder and low temperature binder can be 1-10: 0.1-2: 0.1-2. For example, it can be 1-8: 0.2-2: 0.1-2; 1-10: 0.1-2: 0.1-1; 1-10: 0.2-1: 0.1-1; 1-10: 0.5-2: 0.1-1; 3-10: 1-2: 0.1-1; 10: 2: 1; 10: 1: 0.5; 5: 0.5: 0.2; 5: 1: 1; 2: 0.5: 0.5, etc.

[0061] In an embodiment of the present invention, the amorphous carbon layer is formed by carbonization of a coating agent. The surface of the graphite secondary particles is coated with a coating agent, and the coating agent is filled between adjacent graphite primary particles and adjacent graphite secondary particles. The amorphous carbon layer is formed by carbonization of a coating agent coated on the surface of the graphite secondary particles. The applicable coating agent may be emulsified asphalt or fluidized asphalt.

[0062] In the embodiment of the present invention, the mass ratio of the secondary graphite particles to the coating agent may be 100:(1-100), for example, 100:1, 100:10, 100:30, 100:40, 100:50, 100:60, 100:70, 100:80, 100:90, 100:100, etc.

[0063] The spherical graphite material of the embodiment of the present invention, the low-temperature binder, on the one hand, bonds the graphite primary particles, and on the other hand, cracks during high-temperature shaping, and turns into hard carbon after carbonization. At this time, the high-temperature binder melts and plays a bonding role, bonding the graphite primary particles, and the high-temperature binder turns into soft carbon under carbonization; the coating agent can be emulsified asphalt or fluidized asphalt, which is coated on the surface of the secondary particles and filled in the gaps between the primary particles and the primary particles, the internal pores of a single primary particle, etc., and the adjacent secondary particles are bonded together. The asphalt coated on the surface of the secondary particles forms an amorphous carbon layer after carbonization. The mixture of soft carbon and hard carbon can make the graphite material have high conductivity transport, good mechanical properties and stable morphology, thereby improving the rate performance and cycle stability. The final product spherical graphite material obtained has good isotropy, high density, stable structure, high mechanical strength, and excellent rate performance and cycle stability.

[0064] like Figure 2 As shown, another embodiment of the present invention provides a method for preparing a spherical graphite material, comprising the following steps:

[0065] S1, dispersing graphite primary particles, a high temperature binder, a low temperature binder, and a stabilizer in water to prepare a slurry, and then spray drying to obtain a graphite secondary particle precursor;

[0066] S2, heat-treating the graphite secondary particle precursor under a protective gas atmosphere to obtain graphite secondary particles;

[0067] S3, vacuum impregnating the graphite secondary particles with the coating agent;

[0068] S4, carbonizing the product after vacuum impregnation.

[0069] The embodiment of the present invention proposes a unique secondary particle granulation process for graphite materials. First, the raw materials and auxiliary materials are slurried and then spray-dried to obtain spherical particle granulation products, and then high-temperature shaping is performed to further enhance the granulation effect, improve the structural stability and mechanical properties of the graphite material, and then vacuum impregnation is performed to press the fluidized asphalt into the particle pores produced by high-temperature shaping through atmospheric pressure to densify it, reduce the specific surface and generate a large bonding strength, and finally obtain the desired finished product through a carbonization process. The prepared graphite material exhibits superior fast charging performance, high energy density and excellent cycle stability.

[0070] The spherical graphite material described in the embodiment of the present invention may have a compaction density of 1-2 g / cm 3 , for example, it can be 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , 2.0g / cm 3 , preferably 1.4-1.8g / cm 3 A higher compaction density means that more active materials can be stored per unit volume, thereby increasing the energy density of the battery.

[0071] In the present invention, the tap density (Tap Density or Bulk Density) refers to the maximum packing density of particles in a container after the particles are placed in the container and tapped or vibrated a certain number of times. This process reduces the gaps between the particles, making the particles more closely arranged.

[0072] The OI value of the graphite material described in the embodiment of the present invention is 0.4-1, for example, it can be 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0.

[0073] In the present invention, the OI value refers to the anisotropy index of the material, which is defined by the intensity ratio of a specific peak in an X-ray diffraction (XRD) spectrum, and the OI value = I (004) / I (110). The OI value reflects the degree of anisotropy of the layered structure of the graphite material. The smaller the OI value, the lower the degree of anisotropy of the material and the higher the isotropy, which means that the performance difference of the material in different directions is smaller, which has a positive impact on the rate performance of the material.

[0074] The graphite material of the embodiment of the present invention may have a sphericity of ≥0.75. For example, it may be ≥0.80, ≥0.85, ≥0.90, or ≥0.95. A higher sphericity is beneficial to improving the compaction density and cycle performance of the material, because spherical particles can be more densely packed and reduce the gaps between particles.

[0075] The spherical graphite material of the embodiment of the present invention has a mean particle size D 50It may be 10-30 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, or 30 μm.

[0076] In the present invention, the median particle diameter is usually marked as D 50 , refers to the particle size corresponding to the cumulative frequency of 50% on the particle size distribution curve. For spherical particles, the median particle size is an important parameter that describes the central trend of its particle size distribution and can reflect the average size of the particle group.

[0077] In some embodiments, the graphite primary particles (graphite raw material) in step S1 may have a median particle size D 50 Artificial graphite between 2-10μm. For example, it can be 2-8μm, 2-6μm, 3-8μm, 2-4μm, 2-5μm, 3-6μm, 3-7μm, 3-8μm, 4-8μm, 4-7μm. Smaller median particle size is conducive to the rapid diffusion of lithium ions and improves the rate performance of the material, but it may also increase the formation of SEI film and affect the initial efficiency.

[0078] In some embodiments, the suitable high temperature binder may be one that melts at high temperature (above 500° C.), plays a bonding role and can be used as a binder for the soft carbon donor. For example, it may be asphalt. The median particle size D of the asphalt is 50 It can be 0.5-5 μm, for example, 0.5-4 μm, 0.5-3 μm, 0.5-2 μm, 1-2 μm, 1-3 μm, and preferably between 0.5-3 μm.

[0079] In some embodiments, a suitable low-temperature adhesive is an adhesive with high solubility and can be cross-linked and cured at low temperatures (below 100°C) to play a bonding role. The low-temperature adhesive of the embodiment of the present invention can be one or more of carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) or polyacrylic acid (PAA). The low-temperature adhesive dissolves quickly in the solvent, has high solubility, and can be dissolved in water; has moderate viscosity, is easy to homogenize and maintain the stability of the slurry; can be cross-linked and cured at low temperatures to play a bonding role and bond graphite primary particles; and is cracked into hard carbon when fixed at high temperature.

[0080] The stabilizer suitable for use in the embodiment of the present invention may be one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran, polyethylene oxide or polypropylene oxide. For example, it may be polyethylene glycol (PEG), preferably PEG2000 or PEG1500 or PEG1000. The polyethylene glycol in the embodiment of the present invention is used to stabilize the slurry and increase the probability of ball formation.

[0081] In step S1, the mass ratio of graphite primary particles, high temperature binder, low temperature binder, stabilizer and water can be 1-10: 0.1-2: 0.1-2: 0.1-2: 1-100. For example, it can be 1-8: 0.1-2: 0.1-2: 0.1-2: 1-100; 1-10: 0.1-2: 0.1-1: 0.1-2: 1-100; 1-10: 0.2-1: 0.1-1: 0.1-2: 1-100; 1-10: 0.5-2: 0.1-1: 0.5-2: 1-100; 3-10: 1-2: 0.1-1: 0.1-1: 1-100, etc.

[0082] In the present invention, the low-temperature binder acts synergistically with the high-temperature binder and the stabilizer. The low-temperature binder, on the one hand, stabilizes the slurry in the process of preparing the slurry, making the slurry more uniform while maintaining a long period of time without sedimentation and stratification. At the same time, it undergoes a curing reaction during the spray drying process to play a bonding role, bonding the primary graphite particles, and can be a hard carbon donor, which is hard carbon after carbonization; the high-temperature binder can be asphalt, which plays a bonding role in the process after spray drying (high-temperature shaping, vacuum impregnation, etc., a process with a temperature higher than 400°C), on the one hand, as a soft carbon donor, and on the other hand, bonding the primary graphite particles; polyethylene glycol is used as a stabilizer to stabilize the slurry and increase the probability of ball formation.

[0083] In some embodiments, step S1 can specifically include first adding a low-temperature binder and polyethylene glycol to water, stirring and dissolving, then adding graphite and asphalt, continuing to stir to form a slurry; and then spray drying to obtain spherical particles of graphite material precursor. In this way, graphite and asphalt can be better dissolved in the slurry system. Graphite, asphalt, low-temperature binder, and polyethylene glycol are dispersed in water to form a uniform slurry, and the prepared slurry is pumped into a spray tower and atomized into tiny droplets by an atomizer. The small droplets are balled under the action of their own surface tension, and the water in the spherical small liquid evaporates rapidly. The low-temperature binder contained in the slurry undergoes a curing reaction at this temperature, so that the particles are firmly bonded together to form spherical particles.

[0084] In some embodiments, the inlet temperature of the spray drying in step S1 is 200-300° C., and the outlet temperature is 100-130° C. A graphite secondary particle precursor can be obtained by spray drying. The precursor is a spherical particle.

[0085] In some embodiments, the heat treatment in step S2 may be performed at a high temperature of 500° C. or above.

[0086] In some embodiments, the heat treatment in step S2 may be a gradient temperature rise heat treatment, with a first stage temperature of 100-300°C and a second stage temperature of 500-1000°C. For example, the first stage temperature may be 100°C, 150°C, 200°C, 250°C, 300°C, etc., and the second stage temperature may be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, etc. In this process, asphalt as a high-temperature binder can play a binder role, bonding graphite primary particles together without entering the internal pores of graphite primary particles, while low-temperature binders weaken or directly disintegrate the bonding between particles due to a large amount of volatilization losses at high temperatures. Low-temperature binders play a bonding role in the spray drying process, which is beneficial for graphite to form particles with small particle size and high sphericity.

[0087] In some embodiments, the heating rate of the heat treatment in step S2 may be 2-10°C / min, for example, 2-5°C / min, 5-10°C / min, 2-8°C / min, etc.

[0088] The first stage time of the heat treatment in step S2 can be 0.5-4h, and the second stage time can be 1-8h. For example, the first stage time can be 0.5-1h, 0.5-2h, 1-2h, 2-4h, 0.5h, 1h, 2h, 3.5h, 4h, etc., and the second stage time can be 1-8h, for example, 1-2h, 1-3h, 1-4h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.

[0089] The heat treatment is performed under a protective gas atmosphere, and the protective gas is nitrogen or an inert gas, for example, one or more of nitrogen, argon, xenon, helium, and neon.

[0090] The heat treatment in step S2 is for high-temperature shaping. On the one hand, it makes the asphalt produce a bonding effect, and the low-temperature adhesive is water-soluble. The risk of disintegration due to dissolution of the adhesive during vacuum impregnation can be avoided through high-temperature curing. On the other hand, useless volatile components are removed, so that the density and bonding strength of the spherical particles can be improved by subsequent impregnation.

[0091] In some embodiments, the mass ratio of the graphite secondary particle precursor after heat treatment in step S3 to the coating agent is 100:(1-100), for example, 100:1, 100:10, 100:30, 100:40, 100:50, 100:60, 100:70, 100:80, 100:90, 100:100, etc.

[0092] The coating agent refers to fluidized asphalt or emulsified asphalt. Fluidized asphalt can be prepared by dissolving asphalt in an organic solvent such as gasoline, diesel, benzene, chloroform or carbon tetrachloride. Emulsified asphalt is a liquid asphalt in which asphalt is dispersed in water containing an emulsifier in a droplet state through heat melting and mechanical action to form an oil-in-water (O / W) type.

[0093] The vacuum impregnation is carried out under a protective gas atmosphere, and the protective gas is nitrogen or an inert gas, for example, one or more of nitrogen, argon, xenon, helium, and neon.

[0094] The vacuum impregnation time may be 0.5-50 h, for example, 1-5 h, 2-5 h, 1-10 h, 0.5-30 h, 0.5-40 h, etc.

[0095] Through vacuum impregnation, fluidized asphalt or emulsified asphalt as a coating agent can be filled into the pores inside the graphite under negative pressure and coated on the graphite surface. It has a certain viscosity and can bond different graphite particles together. After carbonization, the asphalt (fluidized asphalt or emulsified asphalt) becomes amorphous carbon, which makes the graphite dense. The compaction density is improved, and the mass of active substances per unit volume is large, and the volume capacity is high; the surface is coated with carbon, and the specific surface area will decrease. If the specific surface area is large, the contact area with the electrolyte is large, and the area of ​​SEI film is also large, the initial efficiency will be low, and the specific surface area is less than 5m 2 / g is better.

[0096] Step S4: Carbonizing the vacuum impregnated product may be performed in a roller kiln in a protective gas atmosphere. The carbonization temperature may be between 1100 and 1300° C. For example, it may be 1100° C., 1200° C., 1300° C., etc. The carbonization time may be 4 to 24 hours. After carbonization, impurities are discharged while improving the compactness, reducing the activity of the bonding component, and making the particles more stable during use.

[0097] The spherical graphite material of the embodiment of the present invention is a core-shell structure, the shell is an amorphous carbon layer, the core is a graphite secondary particle, the graphite secondary particle is granulated from graphite primary particles, soft carbon and a small amount of hard carbon are distributed between the graphite primary particles, the hard carbon is formed by carbonization of a low-temperature binder, and the soft carbon is formed by carbonization of a high-temperature binder. The graphite material of the embodiment of the present invention has excellent rate performance and cycle stability, can be used as a negative electrode material for a battery, can achieve fast charging while increasing the capacity, and takes into account both fast charging and capacity.

[0098] In another embodiment of the present invention, a negative electrode sheet is provided, comprising the spherical graphite material of any embodiment of the present invention. For example, the spherical graphite material of any embodiment of the present invention can be mixed with a conductive agent (such as carbon black (Surper P)) and a binder (such as NMP (N-methylpyrrolidone)) to obtain a slurry, which is then coated on a copper sheet (such as copper foil).

[0099] In yet another embodiment, a battery is provided, comprising the negative electrode sheet according to any embodiment of the present invention.

[0100] The spherical graphite material and preparation method, negative electrode sheet, battery, etc. of the present invention will be further described below in conjunction with specific examples. The materials used in the experiment include graphite raw materials (graphite primary particles), CMC, PEG, asphalt, fluidized asphalt, etc., which can be purchased.

[0101] Example 1

[0102] (1) Dissolve CMC and PEG2000 in pure water at a ratio of 1:2 and stir for 0.5-1.5 h until they are completely dissolved;

[0103] (2) Add the median particle size D to the solution in (1) 50 The graphite primary particles and median particle size D of 5 μm 50 In 1μm asphalt, stir again for 1-2h to make a uniform slurry, in which the ratio of graphite primary particles, asphalt, CMC, PEG2000 and pure water is 2:0.5:0.5:1:20.

[0104] (3) The uniform slurry prepared in (2) is spray-dried, wherein the inlet temperature of the spray-drying is 250° C. and the outlet temperature is 110° C. The finished product of the spray-drying is recorded as a graphite secondary particle precursor.

[0105] (4) The spray-dried finished product is subjected to high-temperature shaping in an Ar atmosphere by gradient heating. The temperature of the first stage is 150°C, and the constant temperature time is 2 hours; the temperature of the second stage is 800°C, and the constant temperature time is 3 hours; the heating rate is 5°C / min. The product of high-temperature shaping is recorded as graphite secondary particles.

[0106] (5) The high temperature set product and fluidized asphalt are vacuum impregnated. The mass ratio of the high temperature set product to the fluidized asphalt is 100:20. The fluidized asphalt is pressed into the pores generated by the high temperature setting by atmospheric pressure, and the vacuum impregnation time is 10 hours.

[0107] (6) The vacuum impregnated product was carbonized in a roller kiln in a N2 atmosphere at a carbonization temperature of 1200°C for 6 h to obtain a median particle size D 50 Spherical artificial graphite secondary particles between 10-30μm.

[0108] Example 2

[0109] The only difference from Example 1 is that PEG2000 in step (1) is replaced by PEG1000.

[0110] Example 3

[0111] The only difference from Example 1 is that the median particle size D of the asphalt in step (2) is 50 is 3μm.

[0112] Example 4

[0113] The only difference from Example 1 is that in step (2), the ratio of graphite primary particles, asphalt, CMC, PEG2000 and pure water is 1:1:0.5:0.5:10.

[0114] Comparative Example 1

[0115] The only difference from Example 1 is that no low-temperature adhesive is added in step (1).

[0116] Comparative Example 2

[0117] The only difference from Example 1 is that the spray drying in step (3) is replaced by vacuum drying.

[0118] Comparative Example 3

[0119] The only difference from Example 1 is that step (4) high temperature shaping is not performed.

[0120] Comparative Example 4

[0121] The only difference from Example 1 is that the second stage temperature in step (4) is 400°C.

[0122] Comparative Example 5

[0123] The only difference from Example 1 is that in step (4), high-temperature shaping is performed in an air atmosphere.

[0124] Comparative Example 6

[0125] The only difference from Example 1 is that step (5) of vacuum impregnation is not performed.

[0126] Comparative Example 7

[0127] The only difference from Example 1 is that step (6) carbonization is not performed.

[0128] Comparative Example 8

[0129] The only difference from Example 1 is that the median particle size D of the primary graphite particles in step (2) is 50is 12μm.

[0130] Performance test experiment

[0131] Compaction density test:

[0132] Test instrument: Sansi Zongheng UTM2103

[0133] Test method: weigh (1±0.0050)g sample, and use the ten-point method to measure at ten pressures of 0.3T, 0.5T, 0.75T, 1.0T, 1.5T, 2.0T, 2.5T, 3.0T, 4.0T, and 5.0T. The holding time is 30s, and then read the data.

[0134] OI value:

[0135] The OI value can be obtained by specific calculation and analysis of the XRD spectrum. The ratio of the (004) diffraction peak intensity (or integrated area) to the (110) diffraction peak intensity (or integrated area) is the orientation degree of graphite, that is, OI = I (004) / I (110). The smaller the OI value, the higher the isotropy.

[0136] Sphericity:

[0137] Testing instruments: optical microscope or scanning electron microscope (SEM).

[0138] Steps: (1) Prepare graphite samples and perform pretreatment (such as drying). (2) Use a microscope to observe the shape and distribution of graphite particles. (3) Select different particles to take images and perform shape analysis. (4) Use image analysis software to measure the major and minor axes of the particles and calculate the sphericity.

[0139] Electrical performance test method: The graphite materials prepared in each embodiment and comparative example are prepared into negative electrode sheets, specifically:

[0140] The above samples were mixed with conductive carbon black (Surper P) and NMP (N-methylpyrrolidone) binder at a mass ratio of 96.5:1.5:2.0 to obtain a slurry, which was then coated on copper foil to form a negative electrode. The prepared negative electrode and lithium metal electrodes were assembled into lithium-ion button cells, and LiPF6 was dissolved in an electrolyte of ethylene carbonate / diethyl carbonate / methyl ethyl carbonate = 2:3:1 at a concentration of 1 mol / L. After the button cell assembly was completed, the capacity, rate performance and cycle performance tests were performed, as shown below:

[0141] (a) 0.1C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min;

[0142] (b) 3C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min; ⑨ 3C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, Let stand for 30 minutes; 0.05C discharge to 0.005V Let stand for 30 minutes; 3C charging to 2V

[0143] (c) 6C discharge specific capacity test steps: ① stand for 5h; ② 0.05C discharge to 0.005V; ③ 0.05mA constant current discharge to 0.005V; ④ stand for 5min; ⑤ 0.01mA constant current discharge to 0.005V; ⑥ stand for 5min; ⑦ 0.1C charge to 2V; ⑧ stand for 5min; ⑨ 6C discharge to 0.005V, ⑩ stand for 30min; 0.1C discharge to 0.005V, Let stand for 30 minutes; 0.05C discharge to 0.005V Let stand for 30 minutes; 6C charging to 2V

[0144] (d) 0.1C 300-cycle capacity retention rate test steps: Same as the 0.1C discharge specific capacity test steps, set the program to cycle 300 times before stopping, and compare its capacity retention rate.

[0145] Data processing: Select 4 data with a range of less than 3 mAh, remove the maximum and minimum values ​​and calculate the average. The data is shown in Table 1.

[0146] Table 1 Comparison of graphite material performance test data

[0147]

[0148] As shown in the data in Table 1, the specific capacity of the graphite material can generally reach about 300mAh / g at a rate of 0.1C. When the specific capacity is above 300, especially above 330mAh / g, it is difficult to increase the specific capacity, and it may be necessary to sacrifice cycle stability or rate performance. The graphite materials of Examples 1-4 of the present invention greatly improve the specific capacity while maintaining good cycle stability and rate performance. The specific capacity is above 330mAh / g and the discharge capacity retention rate is above 90%. The graphite material of the embodiment of the present invention balances long cycle stability and high rate performance, and solves the problem that it is difficult for graphite materials to take into account both fast charging and large capacity.

[0149] In the description of this specification, reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention.

[0150] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Those skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.

[0151] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A spherical graphite material, characterized in that: The spherical graphite material is a core-shell structure, the shell is an amorphous carbon layer, the core is graphite secondary particles, the graphite secondary particles are granulated from graphite primary particles, soft carbon and hard carbon are distributed between the graphite primary particles, the hard carbon is formed by carbonization of a low-temperature binder, and the soft carbon is formed by carbonization of a high-temperature binder.

2. The spherical graphite material according to claim 1, characterized in that: Include one or more of the following characteristics: a1) median particle size D of the spherical graphite material 50 10-30μm; a2) The compacted density of the spherical graphite material is 1-2 g / cm 3 ; a3) The OI value of the spherical graphite material is 0.4-1: a4) the sphericity of the spherical graphite material is ≥0.75; a5) The median particle size D of the graphite primary particles 50 2-8μm; a6) the low-temperature binder is one or more of carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone or polyacrylic acid; a7) the high temperature binder is asphalt; a8) The median particle size D of the high temperature binder 50 0.5-5μm; a9) the amorphous carbon layer is formed by carbonization of a coating agent, and the coating agent is emulsified asphalt or fluidized asphalt; a10) the mass ratio of graphite primary particles, high temperature binder and low temperature binder is 1-10:0.1-2:0.1-2; a11) The mass ratio of graphite secondary particles to coating agent is 100:(1-100).

3. The spherical graphite material according to claim 2, characterized in that: The compaction density of the spherical graphite material is 1.4-1.8 g / cm 3 ; And / or, the sphericity of the spherical graphite material is ≥ 0.80; And / or, the content of hard carbon between the graphite primary particles is lower than the content of soft carbon between the graphite primary particles.

4. A method for preparing a spherical graphite material as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: S1, dispersing graphite primary particles, a high temperature binder, a low temperature binder, and a stabilizer in water to prepare a slurry, and then spray drying to obtain a graphite secondary particle precursor; S2, heat-treating the graphite secondary particle precursor under a protective gas atmosphere to obtain graphite secondary particles; S3, vacuum impregnating the graphite secondary particles with the coating agent; S4. Carbonizing the product after vacuum impregnation to obtain spherical graphite material.

5. The preparation method according to claim 4, characterized in that: In step S1: The low-temperature binder is one or more of carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone or polyacrylic acid; And / or, the high temperature binder is asphalt; And / or, the stabilizer is one or more of polyethylene glycol, polypropylene glycol, polytetrahydrofuran, polyethylene oxide or polypropylene oxide; and / or, the median particle size D of the graphite primary particles 50 2-8μm; And / or, the median particle size D of the high temperature binder 50 0.5-5μm; And / or, the mass ratio of the graphite primary particles, the high-temperature binder, the low-temperature binder, the stabilizer and water is 1-10: 0.1-2: 0.1-2: 0.1-2: 1-100.

6. The preparation method according to claim 4, characterized in that: In step S1: firstly add a low-temperature binder and a stabilizer into water, stir and dissolve, then add graphite primary particles and a high-temperature binder, continue stirring to form a slurry; and then spray dry to obtain a graphite secondary particle precursor.

7. The preparation method according to claim 4, characterized in that: In step S1: the inlet temperature of the spray drying is 200-300°C, and the outlet temperature is 100-130°C.

8. The preparation method according to claim 4, characterized in that: In step S2: The heat treatment is a gradient temperature rise heat treatment, the first stage heat treatment temperature is 100-300°C, the first stage heat treatment time is 0.5-4h, The second stage heat treatment temperature is 500-1000℃, and the second stage heat treatment time is 1-8h; And / or, in step S2, the heating rate of the heat treatment is 2-10°C / min; And / or, in step S2, the heat treatment is performed under a protective gas atmosphere, and the protective gas is one or more of nitrogen, argon, xenon, helium, and neon.

9. The preparation method according to claim 4, characterized in that: In step S3: the vacuum impregnation is performed under a protective gas atmosphere, wherein the protective gas is one or more of nitrogen, argon, xenon, helium, and neon; And / or, the coating agent is emulsified asphalt or fluidized asphalt, and the fluidized asphalt is prepared by dissolving asphalt in gasoline, diesel, benzene, chloroform or carbon tetrachloride; and / or, the mass ratio of the graphite secondary particles to the coating agent is 100:(1-100); And / or, the vacuum impregnation time is 0.5-50h.

10. The preparation method according to claim 4, characterized in that: In step S4, the carbonization is performed under a protective gas atmosphere, and the protective gas is one or more of nitrogen, argon, xenon, helium, and neon; And / or, the carbonization temperature is 1100-1300° C., and the carbonization time is 4-24 h.

11. A negative electrode sheet, characterized in that: The invention comprises the spherical graphite material as described in any one of claims 1 to 3, or comprises the spherical graphite material prepared by the preparation method as described in any one of claims 4 to 10.

12. A lithium ion battery, characterized in that: Comprising the negative electrode sheet as claimed in claim 11.

Citation Information

Cited By

  • Negative electrode material and battery

    CN119315020A

  • Negative electrode material and secondary battery

    WO2026124346A1